[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-465903-105":59,"doc-detail-465903-en":131},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":124,"head_meta":126,"extra_data":128,"updated_unix":130},105,"en","variation-in-alpha-case-thickness-of-ti-xal-castings","Variation in Alpha-Case Thickness of Ti-xAl Castings","","Alpha-case formation, driven by interfacial reactions between molten titanium and oxide molds, limits surface integrity and mechanical performance in titanium castings. This study systematically evaluates how aluminum content (0–52 at%) affects alpha-case formation using plasma arc melting and drop casting with alumina-based molds. Reaction kinetics are assessed via cooling-rate measurements and thermodynamic modeling, while microstructure and composition are characterized through microscopy, hardness, and electron probe microanalysis.",{"@graph":69,"@context":123},[70,84,106],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/variation-in-alpha-case-thickness-of-ti-xal-castings/465903/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/variation-in-alpha-case-thickness-of-ti-xal-castings/465903.png","ImageObject",300,407,{"name":92,"@type":93},"นรินทร์","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-10-31","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":105},"InteractionCounter",{"@type":104},"ViewAction",13,{"@type":107,"mainEntity":108},"FAQPage",[109,115,119],{"name":110,"@type":111,"acceptedAnswer":112},"What is alpha-case formation in titanium casting and why is it important?","Question",{"text":113,"@type":114},"Alpha-case formation is an oxygen-enriched brittle surface layer produced when molten titanium reacts with oxide molds. It degrades mechanical properties by promoting crack initiation and reducing fatigue strength and ductility.","Answer",{"name":116,"@type":111,"acceptedAnswer":117},"How did aluminum content (0–52 at%) influence alpha-case development?",{"text":118,"@type":114},"Increasing aluminum content suppressed alpha-case development. When aluminum exceeded 30 at%, no distinct reaction layer was observed.",{"name":120,"@type":111,"acceptedAnswer":121},"How was the reaction kinetics and alpha-case thickness analyzed in the study?",{"text":122,"@type":114},"The study evaluated reaction kinetics using cooling-rate measurements and thermodynamic modeling, then used microstructural, compositional, and hardness analyses to characterize alpha-case phases and compare calculated thickness with experiments.","https://schema.org",{"og:url":83,"og:type":125,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":127,"canonical":83},"index,follow",{"doc_id":129,"site_id":62},465903,1790813714,{"code":4,"msg":5,"data":132},{"doc_id":129,"user_id":133,"nickname":92,"user_avatar":134,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":135,"file_id":136,"file_url":137,"file_type":138,"file_size":139,"view_count":105,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":140,"language":141,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":142,"faqs":143,"seo_title":144,"seo_description":67,"update_tm":145,"read_time":41,"preview_page_count":19,"preview_urls":146},2336475104957,"https://ap-avatar.wpscdn.com/avatar/22000c4c6bd8a5076e1?x-image-process=image/resize,m_fixed,w_180,h_180&k=1787554080175789136","Article  \nVariation in Alpha-Case Thickness of Ti-xAl Castings  \nByungil Kang 1, Taekyu Ha 1, Seul Lee 2, Youngkyu Ju 2 and Youngjig Kim 1, *  \nAcademic Editors: Tomasz Wróbeland Mariusz Król  \nReceived: 17 November 2025  \nRevised: 11 December 2025  \nAccepted: 15 December 2025  \nPublished: 21 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \n1 Department of Advanced Materials Science and Engineering, Sungkyunkwan University, 2066 Seobu-ro, Jangangu, Suwon 16419, Gyeonggi-do, Republic of Korea; [subs39th@skku.edu](subs39th@skku.edu) (B.K.); [taekyu@skku.edu](taekyu@skku.edu) (T.H.)  \n2 Materials Engineering Team, Hanwha Aerospace, 6, Pangyo-ro, 319beon-gil, Bundang-gu, Seongnam-si 13488, Gyeonggi-do, Republic of Korea; [seul.lee@hanwha.com](seul.lee@hanwha.com) (S.L.); [yk.ju@hanwha.com](yk.ju@hanwha.com) (Y.J.)  \n* [Correspondence: yjk1122@skku.edu](Correspondence: yjk1122@skku.edu)  \nAbstract  \nAlpha-case formation, originating from interfacial reactions between molten titanium and oxide molds, remains a critical issue limiting the surface integrity and mechanical performance of titanium castings. In this study, the effect of aluminum content (0–52 at%) on alpha-case formation was systematically investigated using plasma arc melting and drop casting with alumina-based molds. The reaction kinetics between titanium melts and alumina molds were evaluated through cooling rate measurements and thermodynamic modeling. Microstructural and compositional analyses using optical microscopy, hardness testing, and electron probe microanalysis revealed that increasing aluminum content effectively suppressed alpha-case development. No distinct reaction layer was observed when the aluminum concentration exceeded 30 at% . The alpha-case consisted primarily of Ti 3Al, TiO2, and Ti5Si3 phases, indicating that the molten titanium reacted with both alumina and silica constituents of the mold. Oxygen was identified as the dominant element controlling the reaction depth, consistent with its diffusion behavior across titanium phases. Calculated alpha-case thicknesses showed excellent agreement with experimental measurements, confirming that the reduction in alpha-case depth with increasing aluminum content results from decreased oxygen diffusivity, shorter reaction time, and lower interfacial temperature. These findings establish aluminum addition as a key strategy for minimizing interfacial reactions during titanium investment casting, thereby improving dimensional accuracy and surface quality in high-temperature components.  \nKeywords: titanium alloy; aluminum content; alpha-case formation; investment casting; oxygen diffusion  \n1. Introduction  \nTitanium alloys have been widely used in aerospace, energy, and biomedical applications owing to their high specific strength, corrosion resistance, and superior hightemperature performance. Among various alloy systems, alpha-type and near-alpha titanium alloys are particularly attractive due to their excellent creep resistance, oxidation resistance, and weldability compared to beta-type alloys. Aluminum is known as the most effective alpha-phase stabilizer, improving oxidation and creep resistance at elevated temperatures. Consequently, aluminum-containing titanium alloys such as Ti-6Al-2Sn- 4Zr-2Mo have been extensively employed for compressor blades and disks operating at temperatures up to 565 ◦ C [1–3] . These alloys have therefore been increasingly utilized in advanced turbine components for high-temperature service, where the demand for both  \nweight reduction and high strength is critical. Such trends align with the broader development of γ-TiAl-based intermetallic as next-generation lightweight materials offering comparable high-temperature capability to nickel-based superalloys [4] .  \nHowever, despite these advantages, the pr","cbCaie4z9rgUqje7","https://ap.wps.com/l/cbCaie4z9rgUqje7","pdf",3483511,12,"English","# Abstract\n# Introduction\n## Motivation and background\n## Factors affecting alpha-case formation\n# Experimental Procedure","[{\"question\":\"What is alpha-case formation in titanium casting and why is it important?\",\"answer\":\"Alpha-case formation is an oxygen-enriched brittle surface layer produced when molten titanium reacts with oxide molds. It degrades mechanical properties by promoting crack initiation and reducing fatigue strength and ductility.\"},{\"question\":\"How did aluminum content (0–52 at%) influence alpha-case development?\",\"answer\":\"Increasing aluminum content suppressed alpha-case development. When aluminum exceeded 30 at%, no distinct reaction layer was observed.\"},{\"question\":\"How was the reaction kinetics and alpha-case thickness analyzed in the study?\",\"answer\":\"The study evaluated reaction kinetics using cooling-rate measurements and thermodynamic modeling, then used microstructural, compositional, and hardness analyses to characterize alpha-case phases and compare calculated thickness with experiments.\"}]","Variation in Alpha-Case Thickness of Ti-xAl Castings | PDF",1790770246,[147,151,155,159],{"page_no":8,"url":148,"width":149,"height":150},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/0fa111a09456abdf23f4a19793d9ed38.webp",983,1390,{"page_no":14,"url":152,"width":153,"height":154},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/9aaa8d6d2b5f2205b01e92761362b6cf.webp",982,1388,{"page_no":81,"url":156,"width":157,"height":158},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/392c094374b6fb68b09e3c2b66a9d866.webp",981,1387,{"page_no":19,"url":160,"width":161,"height":162},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/76c005a2f5bc036ec4395e0d2eed5a07.webp",980,1385]