[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-466140-105":59,"doc-detail-466140-en":131},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":124,"head_meta":126,"extra_data":128,"updated_unix":130},105,"en","utilizing-carbonated-reclaimed-water-as-concrete-mixing-water-improved-co2-uptake-and-compressive-strength","Utilizing Carbonated Reclaimed Water as Concrete Mixing Water - Improved CO2 Uptake and Compressive Strength","","This study investigates the carbonation degree of reclaimed water (RW) and its potential use as mixing water for cementitious materials under controlled laboratory conditions using a simplified CO2 injection method. A synthetic reclaimed water system was prepared with a cement-to-sand ratio of 8:2 to reproduce the chemical environment. Thermogravimetric analysis shows high reactivity, achieving 16.8% net CO2 uptake (8.31 g CO2 per kg of RW). Untreated RW slightly reduces flowability and increases superplasticizer demand, while carbonation improves workability and reduces rapid initial setting. Replacing 3% of cement with carbonated RW solids preserves compressive strength, confirming stable CaCO3 retention and dual functionality for mixing and CO2 sequestration.",{"@graph":69,"@context":123},[70,84,106],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/utilizing-carbonated-reclaimed-water-as-concrete-mixing-water-improved-co2-uptake-and-compressive-strength/466140/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/utilizing-carbonated-reclaimed-water-as-concrete-mixing-water-improved-co2-uptake-and-compressive-strength/466140.png","ImageObject",300,407,{"name":92,"@type":93},"Chumphorn","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-10-31","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":105},"InteractionCounter",{"@type":104},"ViewAction",13,{"@type":107,"mainEntity":108},"FAQPage",[109,115,119],{"name":110,"@type":111,"acceptedAnswer":112},"How was carbonation of reclaimed water investigated for use in cementitious mixing water?","Question",{"text":113,"@type":114},"The study used controlled laboratory carbonation with a simplified CO2 injection method and evaluated reclaimed water under designed conditions. A synthetic reclaimed water system was used throughout the assessment.","Answer",{"name":116,"@type":111,"acceptedAnswer":117},"What CO2 uptake performance did the cementitious solids in synthetic reclaimed water achieve?",{"text":118,"@type":114},"Thermogravimetric analysis showed a net CO2 uptake of 16.8%, corresponding to 8.31 g of CO2 sequestered per kilogram of reclaimed water.",{"name":120,"@type":111,"acceptedAnswer":121},"How did carbonation treatment affect concrete performance compared with untreated reclaimed water?",{"text":122,"@type":114},"Untreated reclaimed water slightly reduced flowability and increased superplasticizer demand. Carbonation treatment improved workability and mitigated the rapid initial setting, while 3% replacement with carbonated RW solids did not reduce compressive strength.","https://schema.org",{"og:url":83,"og:type":125,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":127,"canonical":83},"index,follow",{"doc_id":129,"site_id":62},466140,1790813732,{"code":4,"msg":5,"data":132},{"doc_id":129,"user_id":133,"nickname":92,"user_avatar":134,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":135,"file_id":136,"file_url":137,"file_type":138,"file_size":139,"view_count":105,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":46,"language":140,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":67,"update_tm":144,"read_time":31,"preview_page_count":19,"preview_urls":145},2336475401981,"https://ap-avatar.wpscdn.com/avatar/22000c94efd8d5204d?x-image-process=image/resize,m_fixed,w_180,h_180&k=1786935347598174694","Article  \nUtilizing Carbonated Reclaimed Water as Concrete Mixing Water: Improved CO 2 Uptake and Compressive Strength  \nHoon Moon 1, Muhammad Haseeb Zaheer 1,2, Indong Jang 1, Gi-Joon Park 1, Jung-Jun Park 1, Sehee Hong 1 and Namkon Lee 1,2, *  \nAcademic Editors: Jurgita Malaiškiene˙ and Carlos Leiva  \nReceived: 5 December 2025  \nRevised: 16 December 2025  \nAccepted: 19 December 2025  \nPublished: 24 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \n1 Department of Structural Engineering, Korea Institute of Civil Engineering and Building Technology, 283 Goyangdae-ro, Ilsanseo-gu, Goyang-si 10223, Gyeonggi-do, Republic of Korea; [hmoon@kict.re.kr](hmoon@kict.re.kr) (H.M.); [joon7767@kict.re.kr](joon7767@kict.re.kr) (G.-J.P.); [shhong@kict.re.kr](shhong@kict.re.kr) (S.H.)  \n2 Department of Civil and Environmental Engineering, University of Science and Technology, 217 Gajeong-ro, Yuseong District, Daejeon 34113, Republic of Korea  \n* [Correspondence: nklee@kict.re.kr](Correspondence: nklee@kict.re.kr); Tel.: +82-31-910-0583  \nAbstract  \nThis study investigates the carbonation degree of reclaimed water (RW) and its potential use as mixing water for cementitious materials under controlled laboratory conditions using a simplified CO 2 injection method. To reproduce the chemical environment of actual RW, a synthetic reclaimed water (SRW) system with a cement-to-sand ratio of 8:2 was prepared and used throughout the evaluation. Thermogravimetric analysis revealed that the cementitious solids suspended in SRW exhibit high reactivity with CO 2, achieving a net CO2 uptake of 16.8%, equivalent to 8.31 g of CO 2 sequestered per kilogram of RW. The use of untreated RW as mixing water slightly reduced flowability and increased superplasticizer demand compared with distilled water, whereas carbonation treatment of RW improved workability and mitigated the rapid initial setting typically observed with untreated RW. Notably, replacing 3% of the cement with carbonated RW solids did not cause any reduction in compressive strength, indicating that the carbonated solids can be incorporated without compromising mechanical performance. These results confirm that the CaCO3 formed during RW carbonation remains stably retained within mortar and concrete, demonstrating the feasibility of using carbonated RW as a dual-function material—serving both as mixing water and as a medium for CO2 sequestration.  \nKeywords: reclaimed water; carbonation; CO2 uptake; mixing water; compressive strength  \n1. Introduction  \nGlobal efforts to mitigate climate change and achieve carbon neutrality are accelerating, creating a pressing need for the development of carbon-reduction technologies across industrial sectors. Among these, the construction industry is recognized as a major emitter of greenhouse gases, with cement production alone accounting for approximately 7–8% of global CO 2 emissions [1,2] .  \nCement manufacturing requires a high-temperature calcination process at around 1500 ◦ C, during which a considerable volume of CO 2 is released. This process is widely acknowledged as one of the key contributors to the rising levels of greenhouse gases and, consequently, to global climate change [3,4] . Given its indispensable role as a binding material in construction, cement remains essential to infrastructure development. Therefore, the construction industry urgently needs to adopt carbon-reduction strategies that not only reduce CO2 emissions but also facilitate the effective utilization of emitted CO2.  \nDuring the production of ready-mixed concrete, large volumes of wash water are generated, commonly referred to as reclaimed water (RW) . Reclaimed water primarily arises from the washing of batch plant mixers and the cleaning of the interior drums of returned agitator trucks after concrete placemen","cbCaihNX78KLEc9b","https://ap.wps.com/l/cbCaihNX78KLEc9b","pdf",2325983,"English","# Abstract\n# 1. Introduction","[{\"question\":\"How was carbonation of reclaimed water investigated for use in cementitious mixing water?\",\"answer\":\"The study used controlled laboratory carbonation with a simplified CO2 injection method and evaluated reclaimed water under designed conditions. A synthetic reclaimed water system was used throughout the assessment.\"},{\"question\":\"What CO2 uptake performance did the cementitious solids in synthetic reclaimed water achieve?\",\"answer\":\"Thermogravimetric analysis showed a net CO2 uptake of 16.8%, corresponding to 8.31 g of CO2 sequestered per kilogram of reclaimed water.\"},{\"question\":\"How did carbonation treatment affect concrete performance compared with untreated reclaimed water?\",\"answer\":\"Untreated reclaimed water slightly reduced flowability and increased superplasticizer demand. Carbonation treatment improved workability and mitigated the rapid initial setting, while 3% replacement with carbonated RW solids did not reduce compressive strength.\"}]","Utilizing Carbonated Reclaimed Water as Concrete Mixing Water - Improved CO2 Uptake and Compressive Strength | PDF",1790770647,[146,150,154,158],{"page_no":8,"url":147,"width":148,"height":149},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/839d2010e41107551a32c90c4f2b0db6.webp",983,1390,{"page_no":14,"url":151,"width":152,"height":153},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/29ef08f21650977b16d305e4233c189d.webp",982,1388,{"page_no":81,"url":155,"width":156,"height":157},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/9f48a7135ae3f0b9bd0a1ff94d467032.webp",981,1387,{"page_no":19,"url":159,"width":160,"height":161},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/1dd31332ccd6201fca3d98afa69c38b3.webp",980,1385]