[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-514506-105":59,"doc-detail-514506-en":130},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":123,"head_meta":125,"extra_data":127,"updated_unix":129},105,"en","thermal-modification-intensity-of-heat-treated-poplar-wood-part-2-characterization-and-predication-from-outside-to-core-layers","Thermal Modification Intensity of Heat-treated Poplar Wood - Part 2 - Characterization and Predication from Outside to Core Layers","","Thermal modification transition in heat-treated poplar (160–220 °C) is analyzed from surface layers to core layers, extending prior results on the 0–3 mm region. Color changes are quantified using CIELAB, while surface hardness is measured by Shore D and a pressing ball approach; FT-IR is used to assess thermal degradation of wood components. Surface-layer degradation exceeds that of inner layers, and surface color and hardness differ significantly across S0 versus S1–S5.",{"@graph":69,"@context":122},[70,84,105],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/thermal-modification-intensity-of-heat-treated-poplar-wood-part-2-characterization-and-predication-from-outside-to-core-layers/514506/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/thermal-modification-intensity-of-heat-treated-poplar-wood-part-2-characterization-and-predication-from-outside-to-core-layers/514506.png","ImageObject",300,407,{"name":92,"@type":93},"Oliver","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-05","2026-10-06",true,{"@type":102,"interactionType":103,"userInteractionCount":44},"InteractionCounter",{"@type":104},"ViewAction",{"@type":106,"mainEntity":107},"FAQPage",[108,114,118],{"name":109,"@type":110,"acceptedAnswer":111},"What temperature range is used for heat treatment in this study?","Question",{"text":112,"@type":113},"The poplar is heat treated at 160–220 °C.","Answer",{"name":115,"@type":110,"acceptedAnswer":116},"How is surface color change evaluated?",{"text":117,"@type":113},"Color change is evaluated using the CIELAB system.",{"name":119,"@type":110,"acceptedAnswer":120},"Which methods are used to assess hardness and thermal degradation?",{"text":121,"@type":113},"Surface hardness is measured with Shore D and a pressing ball method, and FT-IR is applied to detect thermal degradation of wood components.","https://schema.org",{"og:url":83,"og:type":124,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":126,"canonical":83},"index,follow",{"doc_id":128,"site_id":62},514506,1791390012,{"code":4,"msg":5,"data":131},{"doc_id":128,"user_id":132,"nickname":92,"user_avatar":133,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":134,"file_id":135,"file_url":136,"file_type":137,"file_size":138,"view_count":44,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":139,"language":140,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":67,"update_tm":144,"read_time":41,"preview_page_count":19,"preview_urls":145},8796095461610,"https://ap-avatar.wpscdn.com/davatar_276721f389ce27ea32af1340a28f341c","Yang Li1 , Tao Yao1 , Yong Zhu1 , Shengquan Liu1,2 ,  \nZuju Shu1 , Redžo Hasanagić3 , Leila Fathi4 , Demiao Chu1,2*  \nThermal Modification Intensity of Heat-treated Poplar Wood. Part 2:  \nCharacterization and Predication from Outside to Core Layers  \nIntenzitet toplinske modifikacije topolovine. Dio 2: Karakterizacija i predviđanje od vanjskoga prema unutarnjim slojevima  \nORIGINAL SCIENTIFIC PAPER Izvorni znanstveni rad  \nReceived – prispjelo: 8. 6. 2023.  \nAccepted – prihvaćeno: 25. 9. 2023.  \nUDK: 674.04  \n[https://doi.org/10.5552/drvind.2024.0126](https://doi.org/10.5552/drvind.2024.0126)  \n© 2024 by the author(s) .  \nLicensee University of Zagreb Faculty of Forestry and Wood Technology.  \nThis article is an open access article distributed under the terms and conditions of the  \nCreative Commons Attribution (CC BY) license.  \nABSTRACT • Based on the previous study ofthe heat-treated wood at 0-3 mm surface layer, this study focuses on the transition of thermal modification intensity on 160-220 °C heat-treated poplar from surface to core layers. The color change was evaluated by CIELAB, and surface hardness was detected via Shore D (HD) and pressing ball method (HR); furthermore, the FT-IR was applied to detect the thermal degradation of wood components. The results show that the degradation of cell wall components in the surface layer of heat-treated poplar wood is greater than that in the core layers, and the thermal degradation intensity of the surface layer of the heat-treated poplar wood is greater than that of the other inner layers. Surface color and hardness properties of the heat-treated wood between S0 and S1-S5 test surfaces were significantly different under the same heat treatment conditions; the surface hardness showed an increasing trend, and the HR value oftheH220-2 core layer was 105.71 % higher than that ofthe surface layer. Heat treatment temperature is the main factor affecting the property of wood surface, while the effect of duration is smaller. The hemicellulose content change was mainly related to the degradation intensity on heattreated wood at different locations. An accurate prediction model ofsurface color, hardness, and other properties of the heat-treated wood at different locations was established by Table Curve 3D software.  \nKEYWORDS: heat treatment; modification intensity; transition; hardness; color; surface layer; inner layers; poplar wood  \nSAŽETAK • Prethodno istraživanje toplinski modificiranog drva odnosilo se na površinski sloj od 0 do 3 mm, a ovo se istraživanje bavi prijelazom intenziteta toplinske modifikacije pri 160 – 220 °C s površinskoga prema  \n* Corresponding author  \n1 Authors are researchers at Anhui Agricultural University, School of Materials and Chemistry, Hefei, China. ([https://orcid.org/0009-0006-4785-2595](https://orcid.org/0009-0006-4785-2595))  \n2 Key Lab of National Forestry and Grassland Administration on Wood Quality Improvement & Efficient Utilization, Hefei, China.  \n3 Author is researcher at University ofBihać, Faculty of Technical Engineering, Department of Wood Science and Technology, Bihać, Bosnia and Herzegovina.  \n4 Author is researcher at Shahrekord University, Department of Natural Resources and Earth Science, Shahrekord, Iran.  \n 75 (1) 31-42 (2024) 31  \nunutarnjim slojevima topolovine. Za evaluaciju promjene bojeprimijenjen je CIELab sustav, a tvrdoćapovršine utvrđena je Shore D (HD) metodom i metodom utiskivanja kuglice (HR). Osim toga, procjena toplinske razgradnje spojeva u drvu napravljena je FT-IR spektroskopijom. Rezultati pokazuju da je razgradnja stanične stijenkespojeva drva u površinskom sloju toplinski modificirane topolovine veća nego u središnjim slojevima te daje intenzitet toplinske razgradnjepovršinskog sloja topolovine veći od intenziteta razgradnje ostalih unutarnjih slojeva. Boja površine i svojstva tvrdoće toplinski modificiranog drva između S0 i S1-S5 ispitnih površina značajno su serazlikovali uz jednake uvjete toplinske modifik","cbCaiu23Uz7yhU5j","https://ap.wps.com/l/cbCaiu23Uz7yhU5j","pdf",5331803,12,"English","# ABSTRACT\n# KEYWORDS\n# 1 INTRODUCTION\n## UVOD","[{\"question\":\"What temperature range is used for heat treatment in this study?\",\"answer\":\"The poplar is heat treated at 160–220 °C.\"},{\"question\":\"How is surface color change evaluated?\",\"answer\":\"Color change is evaluated using the CIELAB system.\"},{\"question\":\"Which methods are used to assess hardness and thermal degradation?\",\"answer\":\"Surface hardness is measured with Shore D and a pressing ball method, and FT-IR is applied to detect thermal degradation of wood components.\"}]","Thermal Modification Intensity of Heat-treated Poplar Wood - Part 2 - Characterization and Predication from Outside to Core Layers | PDF",1791300163,[146,150,154,158],{"page_no":8,"url":147,"width":148,"height":149},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/76f4de853e7510bddec34de731713e03.webp",983,1390,{"page_no":14,"url":151,"width":152,"height":153},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/fb0b6953ce836bf157953635d89d439e.webp",982,1388,{"page_no":81,"url":155,"width":156,"height":157},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/c60e474c6ae8881b1222f016eeef4733.webp",981,1387,{"page_no":19,"url":159,"width":160,"height":161},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/5bdf6d600d8034239a05bb7767ecce9c.webp",980,1385]