[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-465884-105":59,"doc-detail-465884-en":131},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":124,"head_meta":126,"extra_data":128,"updated_unix":130},105,"en","the-effect-of-ageing-on-the-mechanical-and-tribological-properties-of-al-zn-mg-alloy","The Effect of Ageing on the Mechanical and Tribological Properties of Al-Zn-Mg Alloy","","Study evaluates how heat treatment—solutionising and ageing between 20–250 °C—changes the microstructure, mechanical response, and tribological behaviour of Al 7075 alloy. Microscopy shows elongated grains and banded precipitate distribution in as-received and naturally aged states, while higher ageing temperatures cause precipitate coarsening and trigger recrystallisation. Hardness peaks at 189 HV after 100 °C/48 h, then declines to 85 HV at 250 °C/4 h; impact strength rises, reaching 26 J/cm² at 250 °C/4 h. T-07 tribology links wear resistance to ageing parameters, with lowest abrasive wear resistance after natural ageing and highest after 250 °C/4 h, indicating hardness–tribology inverse behaviour contrary to Archard’s law.",{"@graph":69,"@context":123},[70,84,106],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/the-effect-of-ageing-on-the-mechanical-and-tribological-properties-of-al-zn-mg-alloy/465884/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/the-effect-of-ageing-on-the-mechanical-and-tribological-properties-of-al-zn-mg-alloy/465884.png","ImageObject",300,407,{"name":92,"@type":93},"วิน","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-11","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":105},"InteractionCounter",{"@type":104},"ViewAction",13,{"@type":107,"mainEntity":108},"FAQPage",[109,115,119],{"name":110,"@type":111,"acceptedAnswer":112},"How does ageing temperature affect microstructure in the alloy?","Question",{"text":113,"@type":114},"As-received and naturally aged conditions show elongated grains and a banded precipitate distribution. Higher ageing temperatures lead to precipitate coarsening and initiation of recrystallisation processes.","Answer",{"name":116,"@type":111,"acceptedAnswer":117},"What ageing condition produced the highest hardness and how did hardness change afterward?",{"text":118,"@type":114},"The highest hardness (189 HV) was obtained after ageing at 100 °C for 48 h. Increasing temperature further caused a systematic hardness decrease down to 85 HV at 250 °C for 4 h.",{"name":120,"@type":111,"acceptedAnswer":121},"How do tribological results relate to heat treatment parameters?",{"text":122,"@type":114},"T-07 tests confirm that wear resistance depends on heat treatment. The lowest relative abrasive wear resistance coefficient (kb = 0.860) occurs after natural ageing, while the highest (kb = 1.216) occurs after ageing at 250 °C for 4 h, showing an inverse relationship with hardness.","https://schema.org",{"og:url":83,"og:type":125,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":127,"canonical":83},"index,follow",{"doc_id":129,"site_id":62},465884,1790814173,{"code":4,"msg":5,"data":132},{"doc_id":129,"user_id":133,"nickname":92,"user_avatar":134,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":135,"file_id":136,"file_url":137,"file_type":138,"file_size":139,"view_count":105,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":140,"language":141,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":142,"faqs":143,"seo_title":144,"seo_description":67,"update_tm":145,"read_time":146,"preview_page_count":19,"preview_urls":147},2336475104736,"https://ap-avatar.wpscdn.com/avatar/22000c4c5e0e5b17e70?x-image-process=image/resize,m_fixed,w_180,h_180&k=1786591360781797222","Article  \nThe Effect of Ageing on the Mechanical and Tribological Properties of Al-Zn-Mg Alloy  \nJakub Papie *, Kacper Le´sny  and Martyna Zemlik *  \nAcademic Editor: Ligang Zhang  \nReceived: 27 October 2025  \nRevised: 16 December 2025  \nAccepted: 22 December 2025  \nPublished: 27 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \nDepartment of Vehicle Engineering, Faculty of Mechanical Engineering, Wrocław University of Science and Technology, Wybrzez˙ e Wyspia ´nskiego 27, 50-370 Wrocław, Poland; [kacper.lesny@pwr.edu.pl](kacper.lesny@pwr.edu.pl)  \n* Correspondence: [267443@student.pwr.edu.pl](267443@student.pwr.edu.pl) (J.P.); [martyna.zemlik@pwr.edu.pl](martyna.zemlik@pwr.edu.pl) (M.Z.)  \nAbstract  \nThe aim of this study was to evaluate the effect of heat treatment, including solutionising and ageing in the temperature range of 20–250 ◦ C, on the microstructural, mechanical, and tribological properties of the Al 7075 alloy. Microscopic analysis revealed that in the as-received condition and after natural ageing, the microstructure is characterised by the presence of elongated grains and a banded distribution of precipitates, whereas higher ageing temperatures lead to their coarsening and the initiation of recrystallisation processes. The highest hardness (189 HV) was obtained after ageing at 100 ◦ C for 48 h, while further increases in temperature caused a systematic decrease in hardness—down to 85 HV at 250 ◦ C for 4 h. Impact tests showed that in the as-received condition, the material reached a value of 7 J/cm2, after natural ageing 15 J/cm2, and the maximum (26 J/cm2 ) was achieved for samples aged at 250 ◦ C for 4 h. Tribological tests conducted using the T-07 method confirmed the dependence of wear resistance on heat treatment parameters—the lowest relative abrasive wear resistance coefficient was observed after natural ageing (kb = 0.860), and the highest after ageing at 250 ◦ C for 4 h (kb = 1.216) . The results obtained indicate that moderate ageing conditions (100–150 ◦ C) favour increased hardness, whereas higher temperatures (200–250 ◦ C) lead to an improvement in impact strength and tribological resistance, which showed an inversely proportional relationship with hardness, contrary to Archard’s law.  \nKeywords: aluminium alloy; abrasive wear; impact strength; heat treatment; 7075  \n1. Introduction  \nA breakthrough moment in the history of the light metal industry occurred in 1886, when the electrolytic process for aluminium production was developed. This made it possible to produce aluminium on an industrial scale, significantly reducing production costs and enabling its widespread use. By the end of the 19th century, aluminium had already found applications in, among others, the manufacture of railway carriages, automotive bodies, and electrical power transmission lines. Since then, aluminium and its alloys have become some of the most important structural materials in modern industry [1] . Aluminium is characterised by a very low density (approx. 2.70 g/cm3 ), combined with a high specific strength (for structural alloys up to 300–600 MPa) and chemical resistance, as well as good thermal (approx. 235 W/m·K) and electrical conductivity (approx. 35–38 MS/m) [2] . These properties, combined with its relatively low price, provide wide possibilities for the material’s application. Aluminium is used, among others, in the food industry, for the construction of chemical equipment, heat exchangers, electrical conductors, lightweight  \nstructures, automotive rims, engine components (e.g., pistons), energy turbines, and in the production of windows and doors [3–6] .  \nAluminium alloys are divided into two main groups: casting alloys and wrought alloys. The latter include the 7xxx series, also known as Al-Zn alloys, which are designed for further heat t","cbCailqAiygPcRRG","https://ap.wps.com/l/cbCailqAiygPcRRG","pdf",7448108,18,"English","# Introduction\n## Heat treatment stages and ageing types\n## Precipitation hardening in 7xxx alloys","[{\"question\":\"How does ageing temperature affect microstructure in the alloy?\",\"answer\":\"As-received and naturally aged conditions show elongated grains and a banded precipitate distribution. Higher ageing temperatures lead to precipitate coarsening and initiation of recrystallisation processes.\"},{\"question\":\"What ageing condition produced the highest hardness and how did hardness change afterward?\",\"answer\":\"The highest hardness (189 HV) was obtained after ageing at 100 °C for 48 h. Increasing temperature further caused a systematic hardness decrease down to 85 HV at 250 °C for 4 h.\"},{\"question\":\"How do tribological results relate to heat treatment parameters?\",\"answer\":\"T-07 tests confirm that wear resistance depends on heat treatment. The lowest relative abrasive wear resistance coefficient (kb = 0.860) occurs after natural ageing, while the highest (kb = 1.216) occurs after ageing at 250 °C for 4 h, showing an inverse relationship with hardness.\"}]","The Effect of Ageing on the Mechanical and Tribological Properties of Al-Zn-Mg Alloy | PDF",1790770213,45,[148,152,156,160],{"page_no":8,"url":149,"width":150,"height":151},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/96fda944ab849dd1aef4615408509ba8.webp",983,1390,{"page_no":14,"url":153,"width":154,"height":155},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/f19398d123c133fbcd5d97d6b198d074.webp",982,1388,{"page_no":81,"url":157,"width":158,"height":159},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/b4aa406757908dfa39f3df4314efb1a2.webp",981,1387,{"page_no":19,"url":161,"width":162,"height":163},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/3bed204b6a73117032059487986828aa.webp",980,1385]