[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-533414-105":59,"doc-detail-533414-en":131},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":124,"head_meta":126,"extra_data":128,"updated_unix":130},105,"en","temperature-and-strain-rate-dependence-of-flow-stress-of-wc-co-cemented-carbides-under-high-temperature-compressive-deformation-research-article","Temperature and strain-rate dependence of flow stress of WC-Co cemented carbides under high temperature compressive deformation - research article","","Investigation clarifies high-temperature deformation mechanisms of WC–Co cemented carbides by measuring strain-rate sensitivity m and apparent activation volume νa for WC-10 and WC-15 mass% Co across 973–1273 K and strain rates from 10−4 to 10−3 s−1 for different WC grain sizes. Coarse-grained carbides show m = 0.03–0.08 and νa rising as stress decreases, reaching 5–10 b3. Fine-grained carbides mimic coarse behavior at high stress, but at low stress m exceeds 0.10 and νa drops to 2–3 b3, indicating dislocation glide versus dislocation creep. Transition stress links to cobalt fraction and WC grain size, guiding suppression of plastic deformation.",{"@graph":69,"@context":123},[70,84,106],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/temperature-and-strain-rate-dependence-of-flow-stress-of-wc-co-cemented-carbides-under-high-temperature-compressive-deformation-research-article/533414/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/temperature-and-strain-rate-dependence-of-flow-stress-of-wc-co-cemented-carbides-under-high-temperature-compressive-deformation-research-article/533414.png","ImageObject",300,407,{"name":92,"@type":93},"Blue Pony","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-19","2026-10-10",true,{"@type":102,"interactionType":103,"userInteractionCount":105},"InteractionCounter",{"@type":104},"ViewAction",11,{"@type":107,"mainEntity":108},"FAQPage",[109,115,119],{"name":110,"@type":111,"acceptedAnswer":112},"What variables were measured to study deformation mechanisms?","Question",{"text":113,"@type":114},"The study measured strain-rate sensitivity m and apparent activation volume νa under high-temperature compression.","Answer",{"name":116,"@type":111,"acceptedAnswer":117},"What trends were observed for coarse-grained versus fine-grained WC–Co carbides?",{"text":118,"@type":114},"Coarse-grained carbides show m between 0.03 and 0.08 with νa increasing as stress decreases, while fine-grained carbides exhibit similar behavior at high stress but higher m and lower νa at low stress.",{"name":120,"@type":111,"acceptedAnswer":121},"How is the transition stress related to material structure?",{"text":122,"@type":114},"The transition stress σtrans, marking the mechanism change from dislocation glide to dislocation creep, relates to cobalt volume fraction and WC grain size.","https://schema.org",{"og:url":83,"og:type":125,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":127,"canonical":83},"index,follow",{"doc_id":129,"site_id":62},533414,1791964708,{"code":4,"msg":5,"data":132},{"doc_id":129,"user_id":133,"nickname":92,"user_avatar":134,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":135,"file_id":136,"file_url":137,"file_type":138,"file_size":139,"view_count":105,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":44,"language":140,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":67,"update_tm":144,"read_time":145,"preview_page_count":19,"preview_urls":146},962090760266,"https://ap-avatar.wpscdn.com/davatar_276721f389ce27ea32af1340a28f341c","International Journal of Refractory Metals and Hard Materials 140 (2026) 107864  \nContents lists available at ScienceDirect  \nInternational Journal of Refractory Metals and Hard Materials  \njournal [homepage:](homepage: www.elsevier.com/locate/IJRMHM)[ www.elsevier.com/locate/IJRMHM](homepage: www.elsevier.com/locate/IJRMHM)  \n| Temperature and strain-rate dependence of flow stress of WC-Co cemented carbides under high temperature compressive deformation☆\u003Cbr>*\u003Cbr>Yu Komamura , Ryu Ichikawa , Shuho Koseki\u003Cbr>Mitsubishi Materials Corporation, Materials Development Section, 1511 Furumagi, Joso-shi, Ibaraki, Japan |  |  | |\n| --- | --- | --- | --- |\n| A R T I C L E I N F O |  | A B S T R A C T |  |\n| Keywords:\u003Cbr>WC–Co cemented carbide Deformation mechanism Thermally activated process Strain-rate jump test |  | In order to clarify the high-temperature deformation mechanisms of WC–Co cemented carbides, the strain-rate sensitivity m and the apparent activation volume νa were measured for WC–10mass%Co and WC–15mass%Co cemented carbides with different WC grain sizes, at strain rates between 10 − 4 and 10 − 3 s − 1 and temperatures between 973 and 1273 K. The coarse-grained cemented carbides exhibited m values of 0.03–0.08, and the apparent activation volume νa increased monotonically with decreasing stress, reaching values of 5–10 b3, where b is the magnitude of the Burgers vector of WC. The fine-grained cemented carbides showed deformation behavior similar to that of the coarse-grained cemented carbides in the high-stress region; however, in the lowstress region, m exceeded 0.10 and νa decreased to 2–3 b3. These results indicate that plastic deformation is mainly governed by dislocation glide in the WC phase in the high-stress region for the fine-grained cemented carbides and over the entire stress range for the coarse-grained cemented carbides, whereas in the low-stress region for the fine-grained cemented carbides, plastic deformation is mainly governed by dislocation creep of the WC phase. Furthermore, a relationship was established between the transition stress σtrans, at which the ratelimiting deformation mechanism changes from dislocation glide to dislocation creep, and the cobalt volume fraction as well as the WC grain size. These relationships provide a useful guideline for material design aimed at suppressing plastic deformation in cemented carbides. |  |\n\n1. Introduction  \nCemented carbides are widely used for cutting tools and wearresistant tools owing to their excellent combination of wear resistance and toughness. During services such as cutting tools or wear-resistant tools, cemented carbides are exposed to severe conditions involving high temperature and high compressive stresses. Such harsh environments can induce macroscopic plastic deformation, which ultimately leads to a reduction in tool life. Moreover, wear mechanisms such as adhesive and abrasive wear are known to involve microscopic plastic deformation processes within the tool material. Therefore, even if a cemented carbide tool does not show macroscopic plastic deformation, suppression of plastic deformation is essential to improve tool life, and in this sense, it is very significant to elucidate the mechanism of plastic deformation of cemented carbides.  \nNumerous studies exist on the deformation mechanisms of cemented carbides, but due to the complexity of the deformation behavior observed in cemented carbides, a unified understanding of these  \nmechanisms has not yet been fully established [1–18]. Since cemented carbides are composite materials, there are theories that claim plastic deformation is governed by the deformation of carbide phase [2,6–10], and binder phase [1,3–5,17]. Both carbide phase and binder phase seem to contribute to the plastic deformation behaviors, but it is difficult to estimate which phase would mainly contribute to plastic deformation behaviors.  \nCollado et al. investigated the hot compression deformation behaviors of WC–7–22mass","cbCaimMVFwbvbmDe","https://ap.wps.com/l/cbCaimMVFwbvbmDe","pdf",5357283,"English","# Introduction\n## Deformation mechanisms in cemented carbides\n# Article context and objectives\n## Scope and measured parameters","[{\"question\":\"What variables were measured to study deformation mechanisms?\",\"answer\":\"The study measured strain-rate sensitivity m and apparent activation volume νa under high-temperature compression.\"},{\"question\":\"What trends were observed for coarse-grained versus fine-grained WC–Co carbides?\",\"answer\":\"Coarse-grained carbides show m between 0.03 and 0.08 with νa increasing as stress decreases, while fine-grained carbides exhibit similar behavior at high stress but higher m and lower νa at low stress.\"},{\"question\":\"How is the transition stress related to material structure?\",\"answer\":\"The transition stress σtrans, marking the mechanism change from dislocation glide to dislocation creep, relates to cobalt volume fraction and WC grain size.\"}]","Temperature and strain-rate dependence of flow stress of WC-Co cemented carbides under high temperature compressive deformation - research article | PDF",1791591032,23,[147,151,155,159],{"page_no":8,"url":148,"width":149,"height":150},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/e2d7630a7742f3c3068fb737f88c989d.webp",983,1310,{"page_no":14,"url":152,"width":153,"height":154},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/843ce37f39cb8733be4d8cf5d872475c.webp",982,1309,{"page_no":81,"url":156,"width":157,"height":158},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/fbe64d76b31e1ba868d91492cf539551.webp",981,1308,{"page_no":19,"url":160,"width":161,"height":162},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/21cbf68d73dd0c5107b6cf962d06e97e.webp",980,1306]