[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-465991-105":59,"doc-detail-465991-en":131},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":124,"head_meta":126,"extra_data":128,"updated_unix":130},105,"en","suppression-mechanism-of-early-age-autogenous-shrinkage-cracking-in-low-water-to-binder-ratio-cement-based-materials-incorporating-ground-granulated-blast-furnace-slag-and-silica-fume","Suppression Mechanism of Early-Age Autogenous Shrinkage Cracking in Low Water-to-Binder Ratio Cement-Based Materials Incorporating Ground Granulated Blast-Furnace Slag and Silica Fume","","Concrete used in water control projects, spillway tunnels, and overflow dams must resist abrasion and cracking under high-velocity flow erosion. Low water-to-binder ratio mixes meet strength needs but show high shrinkage propensity, risking early-age microcracking and reduced long-term safety and durability. This study optimizes performance via synergistic use of GGBS and silica fume in a low water-to-binder system, evaluating compressive strength, drying and autogenous shrinkage, and hydration heat. Results show enhanced strength across ages, delayed onset and reduced rate and ultimate autogenous shrinkage versus pure cement, and retarded heat release that helps mitigate thermal cracking risk. The findings provide regulatory mechanism insight and mix-design support for high-strength, abrasion-resistant, low-shrinkage concrete.",{"@graph":69,"@context":123},[70,84,106],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/suppression-mechanism-of-early-age-autogenous-shrinkage-cracking-in-low-water-to-binder-ratio-cement-based-materials-incorporating-ground-granulated-blast-furnace-slag-and-silica-fume/465991/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/suppression-mechanism-of-early-age-autogenous-shrinkage-cracking-in-low-water-to-binder-ratio-cement-based-materials-incorporating-ground-granulated-blast-furnace-slag-and-silica-fume/465991.png","ImageObject",300,407,{"name":92,"@type":93},"Bintang","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-24","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":105},"InteractionCounter",{"@type":104},"ViewAction",17,{"@type":107,"mainEntity":108},"FAQPage",[109,115,119],{"name":110,"@type":111,"acceptedAnswer":112},"Why does low water-to-binder ratio concrete tend to crack early?","Question",{"text":113,"@type":114},"Lower water content and water consumption during hydration increase autogenous shrinkage under sealed/isothermal conditions. This volume change generates internal stresses and can cause microcracking that harms durability and service life.","Answer",{"name":116,"@type":111,"acceptedAnswer":117},"How do GGBS and silica fume work together in the proposed low water-to-binder system?",{"text":118,"@type":114},"The study investigates synergistic effects of GGBS (20–24%) and silica fume (6–10%) with fixed cement content. Compared with a pure cement system, the blend delays early shrinkage, lowers its rate and ultimate autogenous shrinkage, and improves mechanical performance.",{"name":120,"@type":111,"acceptedAnswer":121},"What evidence indicates reduced risk of both shrinkage and thermal cracking?",{"text":122,"@type":114},"Blends show improved compressive strength at all ages, and shrinkage testing indicates delayed onset and reduced early-age shrinkage. Hydration heat analysis further shows retarded heat release, which helps mitigate thermal cracking risk.","https://schema.org",{"og:url":83,"og:type":125,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":127,"canonical":83},"index,follow",{"doc_id":129,"site_id":62},465991,1790814363,{"code":4,"msg":5,"data":132},{"doc_id":129,"user_id":133,"nickname":92,"user_avatar":134,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":135,"file_id":136,"file_url":137,"file_type":138,"file_size":139,"view_count":105,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":140,"language":141,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":142,"faqs":143,"seo_title":144,"seo_description":67,"update_tm":145,"read_time":36,"preview_page_count":19,"preview_urls":146},962085564381,"https://ap-avatar.wpscdn.com/davatar_6f874abed73319feea01a86fa6f0fab8","Article  \nSuppression Mechanism of Early-Age Autogenous Shrinkage Cracking in Low Water-to-Binder Ratio Cement-Based Materials Incorporating Ground Granulated Blast-Furnace Slag and Silica Fume  \nShuangxi Li 1,*, Guanglang You 1, Gang Yu 2, Chunmeng Jiang 1, Xinguang Xia 3 and Dongzheng Yu 1  \nAcademic Editor: Antonio Caggiano  \nReceived: 29 November 2025  \nRevised: 13 December 2025  \nAccepted: 17 December 2025  \nPublished: 30 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \n1 College of Hydraulic and Civil Engineering, Xinjiang Agricultural University, Urumqi 830052, China  \n2 Xinjiang Tianze Engineering Management Co., Ltd., Shihezi 832003, China  \n3 Xinjiang Yuance Engineering Technology Co., Ltd., Changji 831100, China  \n* [Correspondence: xjlisx123@xjau.edu.cn](Correspondence: xjlisx123@xjau.edu.cn); Tel.: +86-13609912703  \nAbstract  \nIn hydraulic structures such as water control projects, spillway tunnels, and overflow dams that are subjected to high-velocity flow erosion, Concrete is required to exhibit high resistance to abrasion and cracking. While low water-to-binder ratio concrete can meet strength requirements, its inherent high shrinkage propensity often leads to cracking, seriously compromising long-term safety and durability under severe operating conditions. To address this engineering challenge, this study focuses on optimizing concrete performance through the synergistic combination of slag (GGBS) and silica fume (SF) . This study systematically investigated the effects of incorporating GGBS (20–24%) and SF (6–10%) in a low water-to-binder ratio system with a fixed 70% cement content on key concrete properties. The evaluation was conducted through comprehensive tests including compressive strength, drying shrinkage, autogenous shrinkage, and hydration heat analysis. The results demonstrate that the blended system successfully achieves a synergistic improvement in both “high strength” and “low cracking risk.” Specifically, the incorporation of silica fume significantly enhances the compressive strength at all ages, providing a solid mechanical foundation for resisting high-velocity flow erosion. More importantly, compared to the pure cement system, the blended system not only delays the onset but also reduces the rate of early-age shrinkage, and lowers its ultimate autogenous shrinkage value. This characteristic is crucial for controlling the combined effects of thermal and shrinkage stresses from the source and preventing early-age cracking. Simultaneously, hydration heat analysis reveals that the blended system retards the heat release process, which helps mitigate the risk of thermal cracking. This study elucidates the regulatory mechanism of the GGBS-SF combination and provides a critical mix design basis and theoretical support for producing high-strength, high-abrasion-resistant, and low-shrinkage concrete in high-velocity flow environments, offering direct practical implications for engineering applications.  \nKeywords: blended GGBS-SF; low-shrinkage concrete; crack-resistant concrete; highstrength concrete  \n1. Introduction  \nThe development of high-performance and ultra-high-performance concrete (UHPC) represents a significant advancement in modern construction materials, offering exceptional  \nmechanical properties and durability [1] . A fundamental characteristic of these concrete types, particularly ultra-high-performance concrete (UHPC), is a low water-to-binder (w /b) ratio, often below 0.25 . In this study, a w /b of 0.20 was used, which, while at the lower end of the spectrum for such materials, is essential for achieving high compactness and strength [2,3] . However, this very attribute introduces a set of critical challenges, primarily related to the internal moisture environment and the kinetics of cement hydration. The r","cbCaivuF7krPVEbC","https://ap.wps.com/l/cbCaivuF7krPVEbC","pdf",2118958,16,"English","# Abstract\n# Keywords\n# Introduction","[{\"question\":\"Why does low water-to-binder ratio concrete tend to crack early?\",\"answer\":\"Lower water content and water consumption during hydration increase autogenous shrinkage under sealed/isothermal conditions. This volume change generates internal stresses and can cause microcracking that harms durability and service life.\"},{\"question\":\"How do GGBS and silica fume work together in the proposed low water-to-binder system?\",\"answer\":\"The study investigates synergistic effects of GGBS (20–24%) and silica fume (6–10%) with fixed cement content. Compared with a pure cement system, the blend delays early shrinkage, lowers its rate and ultimate autogenous shrinkage, and improves mechanical performance.\"},{\"question\":\"What evidence indicates reduced risk of both shrinkage and thermal cracking?\",\"answer\":\"Blends show improved compressive strength at all ages, and shrinkage testing indicates delayed onset and reduced early-age shrinkage. Hydration heat analysis further shows retarded heat release, which helps mitigate thermal cracking risk.\"}]","Suppression Mechanism of Early-Age Autogenous Shrinkage Cracking in Low Water-to-Binder Ratio Cement-Based Materials Incorporating Ground Granulated Blast-Furnace Slag and Silica Fume | PDF",1790770383,[147,151,155,159],{"page_no":8,"url":148,"width":149,"height":150},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/7a52dcec8c62929213534114658a54ac.webp",983,1390,{"page_no":14,"url":152,"width":153,"height":154},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/f267b6ac1ac0fb45847e24aa871347e4.webp",982,1388,{"page_no":81,"url":156,"width":157,"height":158},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/9e06d78279cdc43f5bd1c142a44f8539.webp",981,1387,{"page_no":19,"url":160,"width":161,"height":162},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/fd8111b6245908403c46c9dac481fab1.webp",980,1385]