[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-466257-105":59,"doc-detail-466257-en":130},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":123,"head_meta":125,"extra_data":127,"updated_unix":129},105,"en","structureproperty-relationship-in-ultra-thin-copper-foils-nanotwinned-to-fine-grained-microstructures-from-nanotwinned-to-fine-grained-microstructures","Structure–Property Relationship in Ultra-Thin Copper Foils - Nanotwinned to Fine-Grained Microstructures - From Nanotwinned to Fine-Grained Microstructures","","This study systematically investigates thickness-dependent mechanical properties of electroplated copper foils with fine-grained (FG-Cu) and columnar nanotwinned (NT-Cu) microstructures. Tensile testing across 5–30 µm shows NT-Cu maintains superior mechanical stability, with substantially smaller reductions in ultimate tensile strength (UTS) and yield strength (YS) than FG-Cu. For FG-Cu, UTS increases from 651 MPa at 30 µm to 792 MPa at 5 µm, while NT-Cu rises only from 624 to 663 MPa over the same range. Microstructural analysis attributes this to stable columnar grains and minimal grain growth, supporting consistent performance across varying foil thicknesses.",{"@graph":69,"@context":122},[70,84,105],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/structureproperty-relationship-in-ultra-thin-copper-foils-nanotwinned-to-fine-grained-microstructures-from-nanotwinned-to-fine-grained-microstructures/466257/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/structureproperty-relationship-in-ultra-thin-copper-foils-nanotwinned-to-fine-grained-microstructures-from-nanotwinned-to-fine-grained-microstructures/466257.png","ImageObject",300,407,{"name":92,"@type":93},"Cipher","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-01","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":44},"InteractionCounter",{"@type":104},"ViewAction",{"@type":106,"mainEntity":107},"FAQPage",[108,114,118],{"name":109,"@type":110,"acceptedAnswer":111},"How does foil thickness affect the tensile properties of FG-Cu versus NT-Cu?","Question",{"text":112,"@type":113},"Tensile testing across 5–30 µm shows NT-Cu has much smaller thickness-induced decreases in both ultimate tensile strength and yield strength than FG-Cu.","Answer",{"name":115,"@type":110,"acceptedAnswer":116},"What UTS values are reported for FG-Cu and NT-Cu at 5 µm and 30 µm?",{"text":117,"@type":113},"For FG-Cu, UTS is 651 MPa at 30 µm and increases to 792 MPa at 5 µm. For NT-Cu, UTS rises from 624 MPa at 30 µm to 663 MPa at 5 µm.",{"name":119,"@type":110,"acceptedAnswer":120},"Why does NT-Cu maintain more stable strength across thicknesses?",{"text":121,"@type":113},"Microstructural analysis indicates NT-Cu preserves a stable columnar grain structure with minimal grain growth, resisting strength loss driven by thickness changes.","https://schema.org",{"og:url":83,"og:type":124,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":126,"canonical":83},"index,follow",{"doc_id":128,"site_id":62},466257,1791169533,{"code":4,"msg":5,"data":131},{"doc_id":128,"user_id":132,"nickname":92,"user_avatar":133,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":134,"file_id":135,"file_url":136,"file_type":137,"file_size":138,"view_count":44,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":139,"language":140,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":67,"update_tm":144,"read_time":145,"preview_page_count":19,"preview_urls":146},687208528416,"https://ap-avatar.wpscdn.com/davatar_9964176cb1d06d4a9deccf72a44ae3dc","Article  \nStructure–Property Relationship in Ultra-Thin Copper Foils: From Nanotwinned to Fine-Grained Microstructures  \nFu-Chian Chen, Dinh-Phuc Tran  and Chih Chen *  \nAcademic Editors: Zine El  \nAbiddine Fellah and Aivaras Kareiva  \nReceived: 18 October 2025  \nRevised: 14 December 2025  \nAccepted: 18 December 2025  \nPublished: 21 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \nDepartment of Materials Science and Engineering, National Yang Ming Chiao Tung University, Hsinchu 300093,  \nTaiwan; [fuchianchen.mse@gmail.com](fuchianchen.mse@gmail.com) (F.-C.C.); [trandinhphuc1508@gmail.com](trandinhphuc1508@gmail.com) (D.-P.T.)  \n* Correspondence: [chihchen@nycu.edu.tw](chihchen@nycu.edu.tw)  \nAbstract  \nThis study systematically investigates the thickness-dependent mechanical properties of electroplated copper foils with fine-grained (FG-Cu) and columnar nanotwinned (NT-Cu) microstructures. Tensile testing across a thickness range of 5–30 µm revealed that NT-Cu exhibits superior mechanical stability, with significantly lower reductions in both ultimate tensile strength (UTS) and yield strength (YS) compared to FG-Cu. The UTS of the 30 µm thick FG-Cu foil was measured at 651 MPa, increasing to 792 MPa at a thickness of 5 µm. In contrast, the UTS of NT-Cu foils only rose from 624 MPa at 30 µm to 663 MPa at 5 µm. A similar trend was observed for the YS. Microstructural analysis confirmed that NT-Cu maintains a stable columnar grain structure with minimal grain growth, contributing to its resistance to thickness-induced strength loss. These findings highlight NT-Cu as a promising candidate for applications requiring consistent mechanical performance across varying foil thicknesses.  \nKeywords: Cu foil; mechanical properties; nanotwinned Cu; columnar grain Cu; fine grained Cu  \n1. Introduction  \nCopper foils play a critical role in a wide range of modern technologies, including flexible electronics [1], microelectronics [2], printed circuit boards [3], and energy storage systems [4] . Their excellent electrical and thermal conductivity, combined with favorable mechanical properties, make them ideal for use as interconnects in advanced packaging [5], flexible circuits in wearable devices [6,7], current collectors in lithium-ion batteries (LIBs) [8] . As applications diversify, the required thickness of copper foils spans a broad range—from ultra-thin foils (\u003C10 µm) for foldable displays [9,10] and stretchable electronics [11,12], to thicker variants (>20 µm) for structural interconnects and battery components. This wide thickness spectrum presents a key engineering challenge: ensuring that the mechanical properties of copper foils remain stable across different thicknesses to support process compatibility, structural reliability, and long-term performance.  \nHowever, the mechanical behavior of copper foils is highly dependent on both their thickness and microstructure. When the foil becomes thinner [13], size-dependent deformation mechanisms such as grain boundary sliding [14], and surface/interface effects [15,16] become increasingly dominant, often leading to significant variations in strength and ductility. To meet industrial requirements, copper foils must exhibit mechanical robustness, defined as minimal variation in tensile or yield strength with changing thickness. Achieving such consistency is particularly challenging with conventional polycrystalline copper.  \nTo enhance the mechanical performance of copper, several classical strengthening mechanisms are commonly employed: grain refinement [17], work hardening [18], precipitation hardening [19], and solid solution strengthening [20] . Nanotwin strengthening has recently been recognized as a fifth and distinct mechanism. Nanotwinned copper (NT-Cu), characterized by high-density nanoscale twin boundaries, o","cbCaihnVgsdJzp95","https://ap.wps.com/l/cbCaihnVgsdJzp95","pdf",9656714,15,"English","# 1. Introduction\n## Background and applications\n## Thickness and microstructure dependence\n## Strengthening mechanisms and nanotwin concept\n## Research gaps\n## Study approach","[{\"question\":\"How does foil thickness affect the tensile properties of FG-Cu versus NT-Cu?\",\"answer\":\"Tensile testing across 5–30 µm shows NT-Cu has much smaller thickness-induced decreases in both ultimate tensile strength and yield strength than FG-Cu.\"},{\"question\":\"What UTS values are reported for FG-Cu and NT-Cu at 5 µm and 30 µm?\",\"answer\":\"For FG-Cu, UTS is 651 MPa at 30 µm and increases to 792 MPa at 5 µm. For NT-Cu, UTS rises from 624 MPa at 30 µm to 663 MPa at 5 µm.\"},{\"question\":\"Why does NT-Cu maintain more stable strength across thicknesses?\",\"answer\":\"Microstructural analysis indicates NT-Cu preserves a stable columnar grain structure with minimal grain growth, resisting strength loss driven by thickness changes.\"}]","Structure–Property Relationship in Ultra-Thin Copper Foils - Nanotwinned to Fine-Grained Microstructures - From Nanotwinned to Fine-Grained Microstructures | PDF",1790770883,38,[147,151,155,159],{"page_no":8,"url":148,"width":149,"height":150},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/c231b072275df89ee95293f05d291963.webp",983,1390,{"page_no":14,"url":152,"width":153,"height":154},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/04fc38a57de3e31fef3dc149b4d9c896.webp",982,1388,{"page_no":81,"url":156,"width":157,"height":158},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/6358c24ce3744e6d5bc00ef267c96585.webp",981,1387,{"page_no":19,"url":160,"width":161,"height":162},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/cadb23b82358edab4700cad19e2bea71.webp",980,1385]