[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"doc-seo-497343-105":3,"detail-sidebar-cat-0-en-105":81,"doc-detail-497343-en":131},{"code":4,"msg":5,"data":6},0,"ok",{"site_id":7,"language":8,"slug":9,"title":10,"keywords":11,"description":12,"schema_data":13,"social_meta":74,"head_meta":76,"extra_data":78,"updated_unix":80},105,"en","standard-method-of-test-for-estimating-damage-tolerance-of-asphalt-binders-using-the-linear-amplitude-sweep-aashto-designation-tp-101-12-ul","Standard Method of Test for Estimating Damage Tolerance of Asphalt Binders Using the Linear Amplitude Sweep - AASHTO Designation: TP 101-12-UL","","Covers a cyclic loading test to determine asphalt binder resistance to fatigue damage using a linear amplitude sweep with a Dynamic Shear Rheometer at the intermediate pavement temperature based on the binder’s performance grade (PG). Asphalt binders may be aged via AASHTO T 240 (RTFOT) and optionally further via AASHTO R 28 (PAV) to represent short- and long-term in-service aging. Includes scope, referenced standards, terminology, test summary, significance, apparatus, and detailed conditioning and sample preparation requirements.",{"@graph":14,"@context":73},[15,34,56],{"@type":16,"itemListElement":17},"BreadcrumbList",[18,23,27,31],{"item":19,"name":20,"@type":21,"position":22},"https://docshare.wps.com","Home","ListItem",1,{"item":24,"name":25,"@type":21,"position":26},"https://docshare.wps.com/document/","Document",2,{"item":28,"name":29,"@type":21,"position":30},"https://docshare.wps.com/document/research-report/","Research & Report",3,{"item":32,"name":10,"@type":21,"position":33},"https://docshare.wps.com/document/standard-method-of-test-for-estimating-damage-tolerance-of-asphalt-binders-using-the-linear-amplitude-sweep-aashto-designation-tp-101-12-ul/497343/",4,{"url":32,"name":10,"@type":35,"image":36,"author":41,"headline":10,"publisher":44,"fileFormat":47,"inLanguage":8,"description":12,"dateModified":48,"datePublished":49,"encodingFormat":47,"isAccessibleForFree":50,"interactionStatistic":51},"DigitalDocument",{"url":37,"@type":38,"width":39,"height":40},"https://docshare.wps.com/thumbnails/standard-method-of-test-for-estimating-damage-tolerance-of-asphalt-binders-using-the-linear-amplitude-sweep-aashto-designation-tp-101-12-ul/497343.png","ImageObject",300,407,{"name":42,"@type":43},"Muffet","Person",{"url":19,"name":45,"@type":46},"DocShare","Organization","application/pdf","2026-11-16","2026-10-02",true,{"@type":52,"interactionType":53,"userInteractionCount":55},"InteractionCounter",{"@type":54},"ViewAction",13,{"@type":57,"mainEntity":58},"FAQPage",[59,65,69],{"name":60,"@type":61,"acceptedAnswer":62},"What does the linear amplitude sweep test measure for an asphalt binder?","Question",{"text":63,"@type":64},"It measures the binder’s damage characteristics and fatigue resistance by applying cyclic shear loading with systematically increasing amplitudes at a constant frequency and using rheological properties plus amplitude-sweep results.","Answer",{"name":66,"@type":61,"acceptedAnswer":67},"Which aging procedures can be used before testing?",{"text":68,"@type":64},"Short-term aging uses AASHTO T 240 (RTFOT); long-term simulation uses AASHTO R 28 (PAV) after T 240, depending on the desired aging level.",{"name":70,"@type":61,"acceptedAnswer":71},"How is the rheometer testing sample prepared and conditioned?",{"text":72,"@type":64},"The sample is prepared following AASHTO T 315 for 8-mm plates with temperature control per the same requirements; conditioning follows AASHTO T 240 for short-term performance or T 240 followed by R 28 for long-term performance.","https://schema.org",{"og:url":32,"og:type":75,"og:title":10,"og:site_name":45,"og:description":12},"article",{"robots":77,"canonical":32},"index,follow",{"doc_id":79,"site_id":7},497343,1791159976,{"code":4,"msg":82,"data":83},"success",[84,88,92,96,101,106,111,115,120,123,127],{"id":22,"doc_module":4,"doc_module_name":25,"category_name":85,"show_sort_weight":86,"slug":87},"Story & Novel",90,"story-novel",{"id":26,"doc_module":4,"doc_module_name":25,"category_name":89,"show_sort_weight":90,"slug":91},"Literature",80,"literature",{"id":33,"doc_module":4,"doc_module_name":25,"category_name":93,"show_sort_weight":94,"slug":95},"Exam",70,"exam",{"id":97,"doc_module":4,"doc_module_name":25,"category_name":98,"show_sort_weight":99,"slug":100},5,"Comic",60,"comic",{"id":102,"doc_module":4,"doc_module_name":25,"category_name":103,"show_sort_weight":104,"slug":105},6,"Technology",50,"technology",{"id":107,"doc_module":4,"doc_module_name":25,"category_name":108,"show_sort_weight":109,"slug":110},7,"Healthcare",40,"healthcare",{"id":112,"doc_module":4,"doc_module_name":25,"category_name":29,"show_sort_weight":113,"slug":114},8,30,"research-report",{"id":116,"doc_module":4,"doc_module_name":25,"category_name":117,"show_sort_weight":118,"slug":119},9,"Religion & Spirituality",20,"religion-spirituality",{"id":118,"doc_module":4,"doc_module_name":25,"category_name":121,"show_sort_weight":118,"slug":122},"World Cup","world-cup",{"id":124,"doc_module":4,"doc_module_name":25,"category_name":125,"show_sort_weight":124,"slug":126},10,"Lifestyle","lifestyle",{"id":128,"doc_module":4,"doc_module_name":25,"category_name":129,"show_sort_weight":97,"slug":130},19,"General","general",{"code":4,"msg":82,"data":132},{"doc_id":79,"user_id":133,"nickname":42,"user_avatar":134,"doc_module":4,"category_id":112,"category_name":29,"doc_title":10,"doc_description":12,"doc_content":135,"file_id":136,"file_url":137,"file_type":138,"file_size":139,"view_count":55,"is_deleted":4,"is_public":22,"is_downloadable":22,"audit_status":22,"page_count":112,"language":140,"language_code":8,"site_id":7,"html_lang":8,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":12,"update_tm":144,"read_time":118,"preview_page_count":33,"preview_urls":145},962090768927,"https://ap-avatar.wpscdn.com/davatar_085a072bc5b1113ac321206ff7593b45","| Standard Method of Test for\u003Cbr>Estimating Damage Tolerance of Asphalt Binders Using the Linear Amplitude Sweep\u003Cbr>AASHTO Designation: TP 101-12-UL |  |\n| --- | --- |\n| 1.\u003Cbr>1.1. | SCOPE\u003Cbr>This test method covers how to determine asphalt binders’ resistance to fatigue damage by means of cyclic loading employing systematically, linearly increasing load amplitudes. The amplitude sweep is conducted using the Dynamic Shear Rheometer at the intermediate pavement temperature determined from the performance grade (PG) of the asphalt binder. The test method can be used with binder aged using AASHTO T 240 (RTFOT) and AASHTO R 28 (PAV) to simulate the estimated aging for inservice asphalt pavements. |\n| 1.2.\u003Cbr>1.3. | The values stated in SI units are to be regarded as the standard.\u003Cbr>This standard does not purport to address all of the safety problems, if any, associated with its use. It is the responsibility of the user of this standard to establish appropriate safety and health practicesand determine the applicability of regulatory limitations prior to use. |\n| 2. | REFERENCED DOCUMENTS |\n| 2.1. | AASHTO Standards:\u003Cbr>M 320, Standard Specification for Performance-Graded Asphalt Binder\u003Cbr>T 240, Standard Method of Test for Effect of Heat and Air on a Moving Film of Asphalt Binder (Rolling Thin-Film Oven Test)\u003Cbr>R 28, Standard Practice for Accelerated Aging of Asphalt Binder Using a Pressurized Aging Vessel (PAV)\u003Cbr>T 315, Standard Method of Test for Determining the Rheological Properties of Asphalt Binder Using a Dynamic Shear Rheometer (DSR) |\n| 2.2. | ASTM Standards:\u003Cbr>D 8, Standard Terminology Relating to Materials for Roads and Pavements\u003Cbr>D 2872, Standard Test Method for Effect of Heat and Air on a Moving Film of Asphalt (Rolling ThinFilm Oven Test)\u003Cbr>D 6521, Standard Practice for Accelerated Aging of Asphalt Binder Using a Pressurized Aging Vessel (PAV)\u003Cbr>D 7175, Standard Test Method for Determining the Rheological Properties of Asphalt Binder Using a Dynamic Shear Rheometer |\n\n3. TERMINOLOGY  \n3.1 Definitions  \n3.1.1 Definitions of terms used in this practice may be found in Terminology D 8, determined from common English usage, or combinations of both.  \n\n| 4.\u003Cbr>4.1 | SUMMARY OF TEST METHOD\u003Cbr>Asphalt binder is first aged using Test Method AASHTO T 240 (ASTM D 2872) (RTFOT) to represent short-term aging of asphalt pavements, or the material may be further aged using AASHTO R 28 (ASTM D 6521-08) prior to testing in order to simulate long-term aging of asphalt pavements. A sample is prepared consistent with Test Method AASHTO T 315 (ASTM D 7175-05) (DSR) using the 8-mm parallel plate geometry with a 2-mm gap setting. The sample is tested in shear using a frequency sweep to determine rheological properties. The sample is then tested using a series of oscillatory load cycles at systematically increasing amplitudes at a constant frequency to cause accelerated fatigue damage. To quantify damage tolerance a rigorous viscoelastic continuum damage approach is used to calculate fatigue resistance from rheological properties and amplitude sweep results. |\n| --- | --- |\n| 5.\u003Cbr>5.1. | SIGNIFICANCE AND USE\u003Cbr>This method is intended to evaluate the ability of an asphalt binder to resist fatigue damage by employing cyclic loading at increasing amplitudes in order to accelerate damage. The characteristics of the rate of damage accumulation in the material can be used to indicate the fatigue performance of the asphalt binder given pavement structural conditions and/or expected amount of traffic loading using predictive modeling techniques. |\n| 6. | APPARATUS |\n| 6.1. | Use the apparatus as specified in T 315. |\n\n7. PROCEDURE  \n7.1. Condition the asphalt binder in accordance with AASHTO T 240 (RTFOT) for short-term performance, or condition the asphalt binder in accordance with AASHTO T 240 (RTFOT) followed by AASHTO R 28 (PAV) for long-term performance.  \n7.2. Sample preparation – The sample for the Linear Amplitude Sweep is prepare","cbCaijjZwUxKhq9B","https://ap.wps.com/l/cbCaijjZwUxKhq9B","pdf",829637,"English","# SCOPE\n## Referenced Documents\n## TERMINOLOGY\n## SUMMARY OF TEST METHOD\n## SIGNIFICANCE AND USE\n## APPARATUS\n## PROCEDURE","[{\"question\":\"What does the linear amplitude sweep test measure for an asphalt binder?\",\"answer\":\"It measures the binder’s damage characteristics and fatigue resistance by applying cyclic shear loading with systematically increasing amplitudes at a constant frequency and using rheological properties plus amplitude-sweep results.\"},{\"question\":\"Which aging procedures can be used before testing?\",\"answer\":\"Short-term aging uses AASHTO T 240 (RTFOT); long-term simulation uses AASHTO R 28 (PAV) after T 240, depending on the desired aging level.\"},{\"question\":\"How is the rheometer testing sample prepared and conditioned?\",\"answer\":\"The sample is prepared following AASHTO T 315 for 8-mm plates with temperature control per the same requirements; conditioning follows AASHTO T 240 for short-term performance or T 240 followed by R 28 for long-term performance.\"}]","Standard Method of Test for Estimating Damage Tolerance of Asphalt Binders Using the Linear Amplitude Sweep - AASHTO Designation: TP 101-12-UL | PDF",1790952441,[146,150,154,158],{"page_no":22,"url":147,"width":148,"height":149},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/9abc50fb4377d538ffd7ee5dc195b34b.webp",983,1272,{"page_no":26,"url":151,"width":152,"height":153},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/79789ceb07d50e087c2d63c8a2b8cd88.webp",982,1270,{"page_no":30,"url":155,"width":156,"height":157},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/085d975d5ccb738f81e0bc38b793b748.webp",981,1269,{"page_no":33,"url":159,"width":160,"height":161},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/6b92cdaac65b95ae6e1afc805f6898a3.webp",980,1268]