[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-511411-105":59,"doc-detail-511411-en":131},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":124,"head_meta":126,"extra_data":128,"updated_unix":130},105,"en","shot-peening-and-roller-burnishing-to-improve-fatigue","Shot Peening and Roller-Burnishing to Improve Fatigue","","The study investigates how shot peening (SP) and roller-burnishing (RB) improve fatigue performance in the (α+β) titanium alloy Ti-6Al-4V, including how treatment conditions influence process-induced residual compressive stresses. A range of Almen intensity and rolling force is applied, with additional mechanical polishing to reduce roughnesses and possible microcracks. Tensile, LCF/HCF fatigue, profilometry roughness, and residual stress-depth profiles via incremental hole drilling are used to relate surface treatment to cyclic deformation behavior and stability.",{"@graph":69,"@context":123},[70,84,106],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/shot-peening-and-roller-burnishing-to-improve-fatigue/511411/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/shot-peening-and-roller-burnishing-to-improve-fatigue/511411.png","ImageObject",300,407,{"name":92,"@type":93},"adawds","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-05","2026-10-06",true,{"@type":102,"interactionType":103,"userInteractionCount":105},"InteractionCounter",{"@type":104},"ViewAction",12,{"@type":107,"mainEntity":108},"FAQPage",[109,115,119],{"name":110,"@type":111,"acceptedAnswer":112},"Why are shot peening and roller-burnishing expected to improve fatigue performance in Ti-6Al-4V?","Question",{"text":113,"@type":114},"They are mechanical surface treatments that can enhance fatigue life by introducing favorable process-induced residual compressive stresses and altering cyclic deformation behavior. The paper emphasizes that the response depends strongly on alloy microstructure and treatment conditions.","Answer",{"name":116,"@type":111,"acceptedAnswer":117},"How were tensile and fatigue specimens prepared for the experiments?",{"text":118,"@type":114},"The alloy Ti-6Al-4V was machined into tensile specimens with defined gauge length and diameter, and into fatigue specimens with hourglass geometry. Tensile tests used threaded cylindrical specimens, while LCF and HCF tests used threaded cylindrical specimens and rotating beam loading, respectively.",{"name":120,"@type":111,"acceptedAnswer":121},"What surface-treatment conditions were compared and why were additional polishing steps included?",{"text":122,"@type":114},"Specimens were compared across electrolytic polishing (EP), shot peening with different Almen intensities (SP), roller-burnishing at different spindle speeds and forces (RB), and combined treatments with mechanical polishing (SP+MP or RB+MP). The additional polishing aimed to reduce process-induced roughnesses and possible microcracks that could affect fatigue behavior.","https://schema.org",{"og:url":83,"og:type":125,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":127,"canonical":83},"index,follow",{"doc_id":129,"site_id":62},511411,1791283886,{"code":4,"msg":5,"data":132},{"doc_id":129,"user_id":133,"nickname":92,"user_avatar":134,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":135,"file_id":136,"file_url":137,"file_type":138,"file_size":139,"view_count":105,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":34,"language":140,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":67,"update_tm":144,"read_time":145,"preview_page_count":19,"preview_urls":146},3985747872983,"https://ap-avatar.wpscdn.com/davatar_994ba38a5ba835b3df7d355c54d3ed8d","# Shot Peening and Roller-Burnishing to Improve Fatigue\n\nResistance of the(α+β)Titanium Alloy Ti-6Al-4V  \nMarcin Kocan¹,Alfred Ostertag²and Lothar Wagner¹  \n¹Chair of Physical Metallurgy and Materials Technology,Technical University of Brandenburg at Cottbus,Cott-bus,Germany²Ecoroll AG,Celle,Germany  \n## 1 Introduction\n\nIt has long been recognized that mechanical surface treatments such as shot peening or rol-ler-burnishing can significantly increase the fatigue performance of structural components.Re-garding the application of light-weight alloys,it is known that titanium and magnesium alloysas opposed to aluminum alloys can respond quite critically to a shot peening treatment.For ex-ample,a very marked over-peening effect was observed on the high-strength magnesium alloyAZ80 [1,2],i.e.,the fatigue life as a function of Almen intensity first dramatically increasedcompared to an electropolished reference followed by a drastic drop as the intensity increased.This sensitivity was attributed to the limited deformability by slip of the hexagonal magnesiumcrystal structure.  \nThe response of titanium alloys to shot peening is reported to strongly depend on many fac-tors,as alloy class(a,(a+β)and metastable β)and its cyclic deformation behavior which inturn determines the cyclic stability of the process-induced residual compressive stresses.For ex-ample,metastable β alloys exhibited only slight improvements of the fatigue performance whilea alloys responded much more beneficially.Further,previous work [3]has shown that the re-sponse of the(α+β)titanium alloy Ti-6Al-7Nb to shot peening and roller-burnishing was clearlyrelated to the mean stress sensitivity of the particular microstructure and crystallographic tex-ture.Conditions with an anomalous mean stress sensitivity [4,5]showed little improvement infatigue performance as opposed to conditions with a normal mean stress sensitivity.  \nThe present investigation was performed on the well known(α+β)titanium alloy Ti-6A1-4Vhaving a typical commercially available mill annealed microstructure.In order to establish opti-mum conditions with regard to fatigue performance,shot peening and roller-burnishing wereperformed using a wide variation in Almen intensity and rolling force,respectively.Additionalpolishing treatments were performed to reduce process-induced roughnesses and microcracks inorder to find out if the fatigue behavior can be further improved.  \n## 2 Experimental\n\nThe(a+β)titanium alloy Ti-6Al-4V was received as Ø10mm rod hot rolled below the betatransus temperature.Prior to rolling,the ingot had been β-forged.The crystallographic texturewas determined by X-ray difraction and will be presented as(0002)pole figure.Tensile and fa-tigue specimens were machined in rolling(RD)direction.Tensile tests were performed on  \nthreaded cylindrical specimens with gage lengths and diameters of 20mm and 4 mm,respec-  \ntively.The initial strain rate was 8.3×10⁻⁴s-¹1.Tensile test results are listed in table 1.  \nTable 1:Tensile properties of Ti-6Al-4V  \n\n| 00.2   | UTS   | El   | RA   |\n| --- | --- | --- | --- |\n| 890 MPa   | 960 MPa   | 13%   | 46%   |\n\nFor fatigue testing,hourglass shaped specimens(3.8 mm gage diameter)were prepared.Spe-cimens were turned (T)under welldefined process conditions.The turning parameters are listedin table 2.  \nTable 2:Turning parameters of the final passes in the as-machined(T)condition  \n\n| Tool bit   | TiN/Al₂O₃/TiCN-CVD coated WC   |\n| --- | --- |\n| Chisel radius   | 0.4 mm   |\n| Infeed   | 0.2 mm   |\n| Feed rate   | 0.15 mm/rev.   |\n| Spindle speed   | 2500 min-1   |\n| Cooling fluid   | oil-water mixture(1:10)   |\n\nOne part of these specimens was electrolytically polished (EP)to serve as further reference.Roughly 100 μm were removed from the surface to ensure that any machining effect that couldmask the results was absent.  \nOthers were shot peened (SP)by means of an injector type machine and a direct pressureblast system for low and high Almen intensities,re","cbCaifXjmX6nzxkC","https://ap.wps.com/l/cbCaifXjmX6nzxkC","pdf",306340,"English","# 1 Introduction\n# 2 Experimental\n# 3 Results and Discussion","[{\"question\":\"Why are shot peening and roller-burnishing expected to improve fatigue performance in Ti-6Al-4V?\",\"answer\":\"They are mechanical surface treatments that can enhance fatigue life by introducing favorable process-induced residual compressive stresses and altering cyclic deformation behavior. The paper emphasizes that the response depends strongly on alloy microstructure and treatment conditions.\"},{\"question\":\"How were tensile and fatigue specimens prepared for the experiments?\",\"answer\":\"The alloy Ti-6Al-4V was machined into tensile specimens with defined gauge length and diameter, and into fatigue specimens with hourglass geometry. Tensile tests used threaded cylindrical specimens, while LCF and HCF tests used threaded cylindrical specimens and rotating beam loading, respectively.\"},{\"question\":\"What surface-treatment conditions were compared and why were additional polishing steps included?\",\"answer\":\"Specimens were compared across electrolytic polishing (EP), shot peening with different Almen intensities (SP), roller-burnishing at different spindle speeds and forces (RB), and combined treatments with mechanical polishing (SP+MP or RB+MP). The additional polishing aimed to reduce process-induced roughnesses and possible microcracks that could affect fatigue behavior.\"}]","Shot Peening and Roller-Burnishing to Improve Fatigue | PDF",1791251633,18,[147,151,155,159],{"page_no":8,"url":148,"width":149,"height":150},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/957c6b26ccf67a431a86f3bc28d4af8a.webp",983,1264,{"page_no":14,"url":152,"width":153,"height":154},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/af7f3bee99bbffa1716b0bd754d3aca5.webp",982,1256,{"page_no":81,"url":156,"width":157,"height":158},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/58cd39c64ab7b8517ad7d60bdadd81f4.webp",981,1254,{"page_no":19,"url":160,"width":161,"height":162},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/df7337cfe9380526ed73358cfe198f8e.webp",980,1251]