[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-469645-105":59,"doc-detail-469645-en":130},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":123,"head_meta":125,"extra_data":127,"updated_unix":129},105,"en","preparation-of-fepanigf-composite-and-study-on-its-interfacial-evaporation-performance","Preparation of Fe/PANI/GF Composite and Study on Its Interfacial Evaporation Performance","","Addressing the global shortage of freshwater resources necessitates the development of efficient and economical photothermal evaporation materials. Herein, an Fe/polyaniline/graphite felt (Fe/PANI/GF) composite was fabricated by combining electrochemical deposition and impregnation. Structural characteristics, photothermal conversion efficiency, and interfacial evaporation performance were systematically investigated. Results demonstrate 95% solar absorption (300–2000 nm) and a rapid surface temperature rise to 60.3 °C under 1 kW m−2 in 5 min, yielding a 2.05 kg m−2 h−1 evaporation rate and 70.3% interfacial evaporation efficiency, attributed to synergistic PANI absorption and Fe coordination-enhanced light capture.",{"@graph":69,"@context":122},[70,84,105],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/preparation-of-fepanigf-composite-and-study-on-its-interfacial-evaporation-performance/469645/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/preparation-of-fepanigf-composite-and-study-on-its-interfacial-evaporation-performance/469645.png","ImageObject",300,407,{"name":92,"@type":93},"pop out","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-10-30","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":52},"InteractionCounter",{"@type":104},"ViewAction",{"@type":106,"mainEntity":107},"FAQPage",[108,114,118],{"name":109,"@type":110,"acceptedAnswer":111},"How was the Fe/PANI/GF composite prepared in this study?","Question",{"text":112,"@type":113},"The Fe/PANI/GF composite was fabricated by combining electrochemical deposition and impregnation.","Answer",{"name":115,"@type":110,"acceptedAnswer":116},"What solar absorption and temperature response did Fe/PANI/GF show?",{"text":117,"@type":113},"It achieved a solar absorption rate of 95% over 300–2000 nm, and under 1 kW m−2 illumination its surface temperature rose from ambient to 60.3 °C within 5 minutes.",{"name":119,"@type":110,"acceptedAnswer":120},"What evaporation performance metrics were reported, and what causes them?",{"text":121,"@type":113},"The composite achieved an evaporation rate of 2.05 kg m−2 h−1 and an interfacial evaporation efficiency of 70.3%, attributed to synergistic broad-spectrum absorption by PANI and enhanced light absorption induced by Fe coordination.","https://schema.org",{"og:url":83,"og:type":124,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":126,"canonical":83},"index,follow",{"doc_id":128,"site_id":62},469645,1791088780,{"code":4,"msg":5,"data":131},{"doc_id":128,"user_id":132,"nickname":92,"user_avatar":133,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":134,"file_id":135,"file_url":136,"file_type":137,"file_size":138,"view_count":52,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":139,"language":140,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":67,"update_tm":144,"read_time":145,"preview_page_count":19,"preview_urls":146},962090760408,"https://ap-avatar.wpscdn.com/davatar_085a072bc5b1113ac321206ff7593b45","Article  \nPreparation of Fe/PANI/GF Composite and Study on Its Interfacial Evaporation Performance  \nJipu Guo 1, Xiaolong Wei 1, Meiyan Wang 2, Xu Li 1, Bin Yan 1, Xiaotong Pan 1, Zhe Zhang 3, Yao Wu 4, Bofang Shi 4 and Honghui Yang 4, *  \nAcademic Editors: Enyi Ye and Piersandro Pallavicini  \nReceived: 31 October 2025  \nRevised: 28 November 2025  \nAccepted: 11 December 2025  \nPublished: 24 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \n1 State Grid (Xi’an) Environmental Protection Technology Center Co., Ltd., Xi’an 710100, China; [jipu_guo@sina.com](jipu_guo@sina.com) (J.G.)  \n2 State Grid Shaanxi Electric Power Company Xi’an Power Supply Company, Xi’an 712000, China  \n3 State Grid Shaanxi Electric Power Co., Ltd. Electric Power Science Research Institute, Xi’an 710100, China  \n4 School of Chemistry, Xi’an Jiaotong University, Xi’an 710049, China; [bofangshi@xjtu.edu.cn](bofangshi@xjtu.edu.cn) (B.S.)  \n* [Correspondence: hhyang@mail.xjtu.edu.cn](Correspondence: hhyang@mail.xjtu.edu.cn)  \nAbstract  \nAddressing the global shortage of freshwater resources necessitates the development of efficient and economical photothermal evaporation materials. Herein, an Fe/polyaniline/graphite felt (Fe/PANI/GF) composite was fabricated by combining electrochemical deposition and impregnation. The structural characteristics, photothermal conversion efficiency, and interfacial evaporation performance of the composite were systematically investigated. Results demonstrate that Fe/PANI/GF exhibits a remarkably high solar absorption rate of 95% across the 300–2000 nm wavelength range. Under 1 kW m−2 illumination, the surface temperature of Fe/PANI/GF rapidly increased from ambient temperature to 60.3 ◦ C within 5 min. The composite achieved an evaporation rate of 2.05 kg m −2 h−1, corresponding to an interfacial evaporation efficiency of 70.3% . This exceptional performance is attributed to the synergistic effect between the broad-spectrum light absorption of PANI and the enhanced light absorption induced by Fe coordination, which collectively promote the photothermal conversion process. This study provides valuable insights for the development of high-performance solar interfacial evaporation materials.  \nKeywords: interfacial evaporation; polyaniline (PANI); graphite felt (GF); photothermal material; seawater desalination  \n1. Introduction  \nEscalating global energy demand, combined with worsening environmental pollution, underscores the critical need for clean and sustainable energy solutions to support the low-carbon transition of human society [1,2] . As an abundant, renewable, and clean energy resource, solar energy has witnessed the maturation of its conversion and utilization technologies into a relatively well-established system via continuous innovation [3,4] . Solar-driven interfacial evaporation (SDIE) technology, leveraging its unique energy utilization mechanism, exhibits significant potential in both academic research and industrial applications. By precisely confining the evaporation process to the water/air interface, SDIE effectively minimizes bulk heat conduction losses inherent in traditional evaporation methods, thereby achieving a substantial improvement in evaporation efficiency. This technology holds considerable promise for applications such as seawater desalination, industrial wastewater treatment, and water resource recycling [5–8] .  \nWithin SDIE systems, photothermal materials serve as the core component, whose performance directly determines the evaporation efficiency and application efficacy of the system. These materials are typically constructed as an absorbing layer at the water/air interface to drive water evaporation via the photothermal conversion effect [6,9] . Recent research efforts have focused on enhancing the solar absorption rate an","cbCailoqACPrgr0R","https://ap.wps.com/l/cbCailoqACPrgr0R","pdf",2753956,11,"English","# 1. Introduction\n## 1.1 Background and motivation\n## 1.2 Photothermal materials and PANI mechanisms\n# 2. Materials and Methods\n## 2.1 Materials and Instruments\n### 2.1.1 Main Materials","[{\"question\":\"How was the Fe/PANI/GF composite prepared in this study?\",\"answer\":\"The Fe/PANI/GF composite was fabricated by combining electrochemical deposition and impregnation.\"},{\"question\":\"What solar absorption and temperature response did Fe/PANI/GF show?\",\"answer\":\"It achieved a solar absorption rate of 95% over 300–2000 nm, and under 1 kW m−2 illumination its surface temperature rose from ambient to 60.3 °C within 5 minutes.\"},{\"question\":\"What evaporation performance metrics were reported, and what causes them?\",\"answer\":\"The composite achieved an evaporation rate of 2.05 kg m−2 h−1 and an interfacial evaporation efficiency of 70.3%, attributed to synergistic broad-spectrum absorption by PANI and enhanced light absorption induced by Fe coordination.\"}]","Preparation of Fe/PANI/GF Composite and Study on Its Interfacial Evaporation Performance | PDF",1790775993,28,[147,151,155,159],{"page_no":8,"url":148,"width":149,"height":150},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/068ee3048bfa3b633cd60f65f616b9bd.webp",983,1390,{"page_no":14,"url":152,"width":153,"height":154},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/c2f2835fe830b40e0d285566ef4ec800.webp",982,1388,{"page_no":81,"url":156,"width":157,"height":158},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/081c76113eac6afcd633ad52ef029144.webp",981,1387,{"page_no":19,"url":160,"width":161,"height":162},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/083125ca1febd2c33cdb5e7d9bffd509.webp",980,1385]