[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-469837-105":59,"doc-detail-469837-en":131},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":124,"head_meta":126,"extra_data":128,"updated_unix":130},105,"en","plasma-enhanced-atomic-layer-deposition-of-alf-3-antireflective-coatings-via-pulse-time-control-of-fluorine-radical-reactions","Plasma-Enhanced Atomic Layer Deposition of AlF 3 Antireflective Coatings via Pulse-Time Control of Fluorine Radical Reactions","","Plasma-enhanced atomic layer deposition (PEALD) is used to grow high-quality aluminum fluoride (AlF 3) antireflective coatings via a safe, HF-free route using trimethylaluminum and SF6 plasma. In situ diagnostics reveal a reaction pathway mediated by a hydrogenterminated fluorinated surface (s-FH). By varying plasma pulse duration, a critical process window is found that balances ligand removal with ion-induced structural damage. In the optimized window, films reach ultra-low impurities and atomically smooth morphology, raising glass optical transmittance to (97.6 ± 0.5)%.",{"@graph":69,"@context":123},[70,84,106],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/plasma-enhanced-atomic-layer-deposition-of-alf-3-antireflective-coatings-via-pulse-time-control-of-fluorine-radical-reactions/469837/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/plasma-enhanced-atomic-layer-deposition-of-alf-3-antireflective-coatings-via-pulse-time-control-of-fluorine-radical-reactions/469837.png","ImageObject",300,407,{"name":92,"@type":93},"OmBimo","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-24","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":105},"InteractionCounter",{"@type":104},"ViewAction",11,{"@type":107,"mainEntity":108},"FAQPage",[109,115,119],{"name":110,"@type":111,"acceptedAnswer":112},"What deposition method is used to create the AlF3 antireflective coatings?","Question",{"text":113,"@type":114},"The study uses plasma-enhanced atomic layer deposition (PEALD) with trimethylaluminum and SF6 plasma.","Answer",{"name":116,"@type":111,"acceptedAnswer":117},"How is HF safety avoided in this PEALD route?",{"text":118,"@type":114},"A safe, HF-free route replaces corrosive HF, using plasma-reactive fluorine species from SF6 instead.",{"name":120,"@type":111,"acceptedAnswer":121},"What variable is tuned to optimize film quality and optical performance?",{"text":122,"@type":114},"The plasma pulse duration is systematically varied to balance fluorination saturation, impurity ligand removal, and ion-induced structural damage.","https://schema.org",{"og:url":83,"og:type":125,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":127,"canonical":83},"index,follow",{"doc_id":129,"site_id":62},469837,1790844813,{"code":4,"msg":5,"data":132},{"doc_id":129,"user_id":133,"nickname":92,"user_avatar":134,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":135,"file_id":136,"file_url":137,"file_type":138,"file_size":139,"view_count":105,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":140,"language":141,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":142,"faqs":143,"seo_title":144,"seo_description":67,"update_tm":145,"read_time":146,"preview_page_count":19,"preview_urls":147},962090893581,"https://ap-avatar.wpscdn.com/davatar_276721f389ce27ea32af1340a28f341c","Article  \nPlasma-Enhanced Atomic Layer Deposition of AlF 3 Antireflective Coatings via Pulse-Time Control of Fluorine Radical Reactions  \nJing Zhang 1, Zhixuan Zhang 2,3, Chia-Hsun Hsu 1,*, Peng Gao 4, Yu Qiu 5, Yuqi Lin 1 and Shui-Yang Lien 1, *  \nAcademic Editor: Christian Mitterer  \nReceived: 29 November 2025  \nRevised: 22 December 2025  \nAccepted: 23 December 2025  \nPublished: 29 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \n1 Xiamen Key Laboratory of Development and Application for Advanced Semiconductor Coating Technology, The School of Opto-Electronic and Communication Engineering, Xiamen University of Technology, Xiamen 361024, China; [2322111025@s.xmut.edu.cn](2322111025@s.xmut.edu.cn) (J.Z.); [2422111017@s.xmut.edu.cn](2422111017@s.xmut.edu.cn) (Y.L.)  \n2 Institute of Optoelectronic Display, National & Local United Engineering Lab of Flat Panel Display Technology, Fuzhou University, Fuzhou 350002, China; [241116005@fzu.edu.cn](241116005@fzu.edu.cn)  \n3 School of Advanced Manufacturing, Fuzhou University, Quanzhou 362200, China  \n4 CAS Key Laboratory of Design a Assembly of Functional Nanostructures, Fujian Provincial Key Laboratory of Nanomaterials, Fujian Institute of Research on the Structure of Matter, Chinese Academy of Sciences, Fuzhou 350002, China; [peng.gao@fjirsm.ac.cn](peng.gao@fjirsm.ac.cn)  \n5 Key Laboratory of Green Perovskites Application of Fujian Province Universities, Fujian Jiangxia University, Fuzhou 350108, China; [yuqiu@fjjxu.edu.cn](yuqiu@fjjxu.edu.cn)  \n* Correspondence: [2019000001@xmut.edu.cn](2019000001@xmut.edu.cn) (C.-H.H.); [sylien@xmut.edu.cn](sylien@xmut.edu.cn) (S.-Y.L.)  \nAbstract  \nPlasma-enhanced atomic layer deposition (PEALD) is used to grow high-quality aluminum fluoride (AlF 3) antireflective coatings via a safe, HF-free route using trimethylaluminum and SF6 plasma. In situ diagnostics reveal a reaction pathway mediated by a hydrogenterminated fluorinated surface (s-FH). By systematically varying the plasma pulse duration, a critical process window is identified that balances efficient ligand removal against ioninduced structural damage. Within this optimized window, the films achieve ultra-low impurity levels and an atomically smooth morphology, increasing the optical transmittance of glass to (97.6 ± 0.5)% . This study establishes a clear link between fundamental plasma kinetics and functional optical performance, providing a robust, non-corrosive strategy for the rational design of metal–fluoride PEALD coatings.  \nKeywords: aluminum fluoride; plasma enhanced atomic layer deposition; antireflective; optical electronics  \n1. Introduction  \nAluminum fluoride (AlF 3) is a compelling dielectric material, distinguished by its ultra-wide bandgap (>10 eV), very low refractive index (~1.3–1.4), and excellent chemical and thermal stability [1–3] . These attributes make it a key enabling material for a variety of advanced technologies, including high-performance antireflective coatings for deepultraviolet optics, gate dielectrics in wide-bandgap electronics, and protective layers for next-generation lithium-ion batteries [4–8] . Realizing these applications, however, demands AlF3 thin films that are not only stoichiometric and highly pure but also conformal and atomically smooth—requirements that are difficult to meet using conventional deposition techniques. Traditional approaches such as physical vapor deposition and chemical vapor deposition (CVD) often exhibit limited conformality, require elevated processing temperatures, or introduce plasma-induced damage, all of which can degrade film quality [9,10] . In contrast, atomic layer deposition (ALD) has emerged as a superior technique, offering angstrom-level thickness control, excellent conformality, and low-temperature processing  \ncapabilities [11–13] . The mo","cbCaivP6ugtqkTei","https://ap.wps.com/l/cbCaivP6ugtqkTei","pdf",3666458,17,"English","# Abstract\n# Keywords\n# 1. Introduction","[{\"question\":\"What deposition method is used to create the AlF3 antireflective coatings?\",\"answer\":\"The study uses plasma-enhanced atomic layer deposition (PEALD) with trimethylaluminum and SF6 plasma.\"},{\"question\":\"How is HF safety avoided in this PEALD route?\",\"answer\":\"A safe, HF-free route replaces corrosive HF, using plasma-reactive fluorine species from SF6 instead.\"},{\"question\":\"What variable is tuned to optimize film quality and optical performance?\",\"answer\":\"The plasma pulse duration is systematically varied to balance fluorination saturation, impurity ligand removal, and ion-induced structural damage.\"}]","Plasma-Enhanced Atomic Layer Deposition of AlF 3 Antireflective Coatings via Pulse-Time Control of Fluorine Radical Reactions | PDF",1790776318,43,[148,152,156,160],{"page_no":8,"url":149,"width":150,"height":151},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/a3aa66b0c82125a15431a2e3abb01693.webp",983,1390,{"page_no":14,"url":153,"width":154,"height":155},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/753fb4ad69ae7362ef81822ac46905fd.webp",982,1388,{"page_no":81,"url":157,"width":158,"height":159},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/8fabc3103f77b8c1111129152b3e9551.webp",981,1387,{"page_no":19,"url":161,"width":162,"height":163},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/9d075c73344d2a1aa9326dfb46762376.webp",980,1385]