[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-462584-105":59,"doc-detail-462584-en":130},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":123,"head_meta":125,"extra_data":127,"updated_unix":129},105,"en","localized-corrosion-by-chromium-nitride-precipitation-in-low-temperature-plasma-nitrided-inconel-718","Localized Corrosion by Chromium Nitride Precipitation in Low-Temperature Plasma-Nitrided Inconel 718","","Inconel 718 is widely used in chloride-bearing environments where localized corrosion resistance is critical. This study evaluates continuous low-temperature plasma nitriding (425 °C, 2 h) effects on microstructure, hardness, and localized corrosion behavior. The treatment formed a nitrided surface layer with hardness up to threefold higher than the untreated alloy and a thickness of 6.1–6.7 µm. X-ray diffraction confirmed CrN precipitation without nitrogen-expanded phases. Cyclic polarization showed corrosion parameter changes were mostly non-significant, except for a twofold increase in corrosion rate and a more than 30 °C average drop in CPT, below 10 °C, indicating compromised localized corrosion resistance.",{"@graph":69,"@context":122},[70,84,105],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/localized-corrosion-by-chromium-nitride-precipitation-in-low-temperature-plasma-nitrided-inconel-718/462584/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/localized-corrosion-by-chromium-nitride-precipitation-in-low-temperature-plasma-nitrided-inconel-718/462584.png","ImageObject",300,407,{"name":92,"@type":93},"Đào","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-06","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":44},"InteractionCounter",{"@type":104},"ViewAction",{"@type":106,"mainEntity":107},"FAQPage",[108,114,118],{"name":109,"@type":110,"acceptedAnswer":111},"What low-temperature plasma nitriding condition was investigated for Inconel 718?","Question",{"text":112,"@type":113},"The study used continuous low-temperature plasma nitriding at 425 °C for 2 hours.","Answer",{"name":115,"@type":110,"acceptedAnswer":116},"How did nitriding affect hardness and the nitrided layer thickness?",{"text":117,"@type":113},"Nitriding produced a surface layer with hardness up to about three times higher than the untreated material, associated with a nitrided layer thickness of 6.1–6.7 µm.",{"name":119,"@type":110,"acceptedAnswer":120},"What changes were observed in localized corrosion behavior after nitriding?",{"text":121,"@type":113},"Cyclic polarization showed non-significant changes in most corrosion parameters, except for a twofold increase in corrosion rate; the critical pitting temperature decreased by more than 30 °C on average, dropping below 10 °C.","https://schema.org",{"og:url":83,"og:type":124,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":126,"canonical":83},"index,follow",{"doc_id":128,"site_id":62},462584,1790818608,{"code":4,"msg":5,"data":131},{"doc_id":128,"user_id":132,"nickname":92,"user_avatar":133,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":134,"file_id":135,"file_url":136,"file_type":137,"file_size":138,"view_count":44,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":139,"language":140,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":67,"update_tm":144,"read_time":145,"preview_page_count":19,"preview_urls":146},1374402968488,"https://ap-avatar.wpscdn.com/davatar_29158cc5080c5b710cf443261637dec0","Article  \nLocalized Corrosion by Chromium Nitride Precipitation in Low-Temperature Plasma-Nitrided Inconel 718  \nJuan Fernando Uribe Cruz 1, Oriana Palma Calabokis 1,2, *, Vladimir Ballesteros-Ballesteros 1, Yamid E. Nuñez de la Rosa 1,2 and Edward Andrés Gil González 1  \nAcademic Editors: Yang Bao, Xinxin Ma and Daniel  \nJohn Blackwood  \nReceived: 20 November 2025  \nRevised: 16 December 2025  \nAccepted: 18 December 2025  \nPublished: 23 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \n1 Faculty of Engineering and Basic Sciences, Fundación Universitaria Los Libertadores, Bogotá 111221, Colombia; [jfuribec@libertadores.edu.co](jfuribec@libertadores.edu.co) (J.F.U.C.); [vladimir.ballesteros@libertadores.edu.co](vladimir.ballesteros@libertadores.edu.co) (V.B.-B.); [yenunezd@libertadores.edu.co](yenunezd@libertadores.edu.co) (Y.E.N.d.l.R.); [eagilg@libertadores.edu.co](eagilg@libertadores.edu.co) (E.A.G.G.)  \n2 Soft Matter Research Center—SOFMAT, Research Center for Rheology and Non-Newtonian Fluids—CERNN, Federal University of Technology–Parana—UTFPR, Curitiba 81280-340, Paraná, Brazil  \n* Correspondence: [opalmac@libertadores.edu.co](opalmac@libertadores.edu.co)  \nAbstract  \nInconel 718 is widely used in chloride-bearing environments where localized corrosion resistance is critical. This study assesses the effect of continuous low-temperature plasma nitriding (425 ◦ C, 2 h) on the microstructure, hardness, and localized corrosion behavior of Inconel 718 . The nitriding treatment produced a surface layer with hardness values up to three times higher than those of the untreated material, associated with a nitrided layer of thickness 6.1–6.7 µm. X-ray diffraction confirmed the precipitation of CrN without the formation of nitrogen-expanded phases. Cyclic polarization tests revealed non-significant changes in the corrosion parameters, except for a two-fold increase in the corrosion rate of nitrided samples. Also, the critical pitting temperature (CPT) decreased by more than 30 ◦ C on average in the nitrided condition, falling below 10 ◦ C. These findings indicate that, although continuous plasma nitriding enhances surface hardening, it significantly compromises the alloy’s resistance to localized corrosion in chloride-rich environments.  \nKeywords: chloride environments; chromium nitride CrN; corrosion resistance; critical pitting temperature; Inconel 718; plasma nitriding  \n1. Introduction  \nInconel 718 is widely recognized for its excellent corrosion resistance and its ability to maintain high mechanical strength under demanding service conditions, making it indispensable in aerospace, petrochemical, and marine environments [1,2] . Despite its robustness, the alloy remains susceptible to localized corrosion, particularly pitting and crevice attack, in chloride-rich media, a limitation that continues to challenge its long-term durability [3,4] .  \nFor that reason, surface engineering has become an important complement to the alloy’s intrinsic properties. Techniques such as boriding, carburizing, and nitriding have been explored over the years [5–7] . Among them, plasma nitriding has gained prominence for nickel-based alloys, including Inconel 718, due to its ability to introduce nitrogen into the surface, forming hardened layers, and inducing beneficial microstructural modifications [8] . Compared with gas or salt-bath nitriding, plasma nitriding offers improved control over layer thickness, reduced thermal distortion, shorter treatment times, and lower environmental impact [9] .  \nHowever, the success of plasma nitriding depends strongly on processing temperature, time, and nitrogen potential. At low temperatures, typically around 400 ◦ C, nitrogen incorporation can produce an expanded austenite layer (γN or S phase), which generally enhances both hardness and c","cbCaihOkaH3kxhGa","https://ap.wps.com/l/cbCaihOkaH3kxhGa","pdf",3234443,15,"English","# Abstract\n# Keywords\n# 1. Introduction","[{\"question\":\"What low-temperature plasma nitriding condition was investigated for Inconel 718?\",\"answer\":\"The study used continuous low-temperature plasma nitriding at 425 °C for 2 hours.\"},{\"question\":\"How did nitriding affect hardness and the nitrided layer thickness?\",\"answer\":\"Nitriding produced a surface layer with hardness up to about three times higher than the untreated material, associated with a nitrided layer thickness of 6.1–6.7 µm.\"},{\"question\":\"What changes were observed in localized corrosion behavior after nitriding?\",\"answer\":\"Cyclic polarization showed non-significant changes in most corrosion parameters, except for a twofold increase in corrosion rate; the critical pitting temperature decreased by more than 30 °C on average, dropping below 10 °C.\"}]","Localized Corrosion by Chromium Nitride Precipitation in Low-Temperature Plasma-Nitrided Inconel 718 | PDF",1790764603,38,[147,151,155,159],{"page_no":8,"url":148,"width":149,"height":150},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/1c2c4383874f2c0bb791c1d16d2829bd.webp",983,1390,{"page_no":14,"url":152,"width":153,"height":154},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/fd704c597187cbdbed117390b0b5fbaf.webp",982,1388,{"page_no":81,"url":156,"width":157,"height":158},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/e1d9cd2936e2187dbda629e71a063b6c.webp",981,1387,{"page_no":19,"url":160,"width":161,"height":162},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/54643045018fb1df58d4c187b03378f1.webp",980,1385]