[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-466199-105":59,"doc-detail-466199-en":131},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":124,"head_meta":126,"extra_data":128,"updated_unix":130},105,"en","laser-power-dependent-microstructural-evolution-and-fracture-mechanisms-in-ti80-titanium-alloy-welds","Laser Power-Dependent Microstructural Evolution and Fracture Mechanisms in Ti80 Titanium Alloy Welds","","Laser welding of 4 mm thick Ti80 alloy under different laser powers examines weld morphology, microstructure and mechanical response. A temperature–stress simulation model is built with ABAQUS and applied at 2520 W and 3000 W, then verified through experiments. Increasing power shifts weld morphology from Y-shaped to X-shaped, altering pore counts for incomplete and complete penetration. EBSD-derived maps (grain boundaries, KAM and GND density) reveal fine acicular α′ phase, while hardness rises to 420–460 HV in the weld zone and ductile fracture is indicated by tensile results at 3000 W.",{"@graph":69,"@context":123},[70,84,106],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/laser-power-dependent-microstructural-evolution-and-fracture-mechanisms-in-ti80-titanium-alloy-welds/466199/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/laser-power-dependent-microstructural-evolution-and-fracture-mechanisms-in-ti80-titanium-alloy-welds/466199.png","ImageObject",300,407,{"name":92,"@type":93},"Nguyễn Văn Học","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-05","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":105},"InteractionCounter",{"@type":104},"ViewAction",15,{"@type":107,"mainEntity":108},"FAQPage",[109,115,119],{"name":110,"@type":111,"acceptedAnswer":112},"How does increasing laser power affect Ti80 weld morphology?","Question",{"text":113,"@type":114},"With higher laser power, the weld morphology changes from Y-shaped to X-shaped. It also modifies the number of pores under incomplete and complete penetration conditions.","Answer",{"name":116,"@type":111,"acceptedAnswer":117},"What microstructural features are observed in the weld zone?",{"text":118,"@type":114},"The weld zone contains fine acicular α′ phase. EBSD analysis generates grain boundary distribution, KAM maps, and GND density maps to characterize microstructural evolution.",{"name":120,"@type":111,"acceptedAnswer":121},"How were simulation results validated and how accurate were they?",{"text":122,"@type":114},"The ABAQUS simulation predicted temperature and stress fields during/after laser welding and was verified using experiments. The predicted maximum longitudinal residual stress matches measurements with an error range of 1.65% to 1.81%.","https://schema.org",{"og:url":83,"og:type":125,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":127,"canonical":83},"index,follow",{"doc_id":129,"site_id":62},466199,1790818623,{"code":4,"msg":5,"data":132},{"doc_id":129,"user_id":133,"nickname":92,"user_avatar":134,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":135,"file_id":136,"file_url":137,"file_type":138,"file_size":139,"view_count":105,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":140,"language":141,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":142,"faqs":143,"seo_title":144,"seo_description":67,"update_tm":145,"read_time":146,"preview_page_count":19,"preview_urls":147},1374402739827,"https://ap-avatar.wpscdn.com/avatar/14000c97e7351f1a627?x-image-process=image/resize,m_fixed,w_180,h_180&k=1787885694763230660","Article  \nLaser Power-Dependent Microstructural Evolution and Fracture Mechanisms in Ti80 Titanium Alloy Welds: A Multi-Scale Investigation  \nChuanbo Zheng 1, Zhanwen Yang 1,*, Guo Yi 1,*, Liuyu Zhang 2, Xiaomeng Zhou 2 and Xinyu Yao 2  \nAcademic Editor: Liyuan Sheng  \nReceived: 21 November 2025  \nRevised: 17 December 2025  \nAccepted: 22 December 2025  \nPublished: 29 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \n1 School of Metallurgy and Engineering, Jiangsu University of Science and Technology, Zhangjiagang 215600, China; [15952802516@139.com](15952802516@139.com)  \n2 Suzhou Sitri Welding Technology Research Institute Co., Ltd., Zhangjiagang 215600, China  \n* [Correspondence: yzw1@foxmail.com](Correspondence: yzw1@foxmail.com) (Z.Y.); [15952879216@139.com](15952879216@139.com) (G.Y.)  \nAbstract  \nThe laser welding of 4 mm thick Ti80 alloy under different powers was analyzed, and the weld morphology, microstructure, and mechanical properties were studied. A simulation model was established based on ABAQUS, and laser welding simulations were conducted using 2520 W and 3000 W laser welding power sources to analyze the temperature field and stress field, which were verified by experiments. The increase in power changed the weld morphology from Y-shaped to X-shaped and affected the number of pores in incomplete and complete penetration. The microstructure in the weld zone presented fine acicular α′ phase. Subsequently, grain boundary distribution maps, Kernel Average Misorientation (KAM) maps, and geometrically necessary dislocation (GND) density maps were generated through electron backscatter diffraction (EBSD) analysis. These comprehensive data visualizations enabled multi-dimensional investigation, establishing and analyzing correlations between laser welding parameters, microstructural evolution, and mechanical properties in Ti80 titanium laser welding. The hardness of the base material was 320 HV to 360 HV, and it increased from 420 HV to 460 HV in the weld zone. At 3000 W, the tensile strength reached 903.12 MPa, and the elongation was 10.40%, indicating ductile fracture. The simulation results accurately predicted the maximum longitudinal residual stress in the weld zone, with an error of 1 .65% to 1 .81% of the measured value.  \nKeywords: Ti80 titanium alloy; laser welding; mechanical properties; simulation  \n1. Introduction  \nIn the 21st century, the ocean has emerged as a critical domain of competition among nations in political, economic, and military spheres. Research into marine science and the development of marine engineering technologies have been elevated to the strategic decision-making level of national policies. Titanium not only possesses high strength and excellent corrosion resistance but also offers a significant lightweight advantage that is absent in other commonly used marine engineering materials. Replacing traditional materials such as stainless steel and aluminum with titanium can substantially extend the service life of marine engineering equipment, reduce maintenance and repair costs, and enhance the safety and reliability of marine operations [1–3] . Furthermore, the corrosion resistance of titanium alloys in marine environments can be significantly enhanced by fabricating surface coatings with superhydrophobic properties [4] .  \nTC4, Ti31, and Ti80 are among the most commonly used titanium alloys in marine engineering. Among these, Ti80, a near-α type titanium alloy, exhibits excellent mechanical properties and superior weldability [5] . Consequently, it finds extensive application in critical components such as large-diameter pressure pipelines, high-pressure vessels, deepsea submersibles, ship pressure hulls, and welded structural components of vessels. Given its widespread use in significant marine engineering projects,","cbCaib9LxrRuPl1p","https://ap.wps.com/l/cbCaib9LxrRuPl1p","pdf",20827943,26,"English","# Abstract\n# Keywords\n# 1. Introduction\n## Titanium for marine engineering applications\n## Welding methods and research gap\n# 2. Experiment and Simulation Modeling Methods\n## 2.1. Materials and Welding","[{\"question\":\"How does increasing laser power affect Ti80 weld morphology?\",\"answer\":\"With higher laser power, the weld morphology changes from Y-shaped to X-shaped. It also modifies the number of pores under incomplete and complete penetration conditions.\"},{\"question\":\"What microstructural features are observed in the weld zone?\",\"answer\":\"The weld zone contains fine acicular α′ phase. EBSD analysis generates grain boundary distribution, KAM maps, and GND density maps to characterize microstructural evolution.\"},{\"question\":\"How were simulation results validated and how accurate were they?\",\"answer\":\"The ABAQUS simulation predicted temperature and stress fields during/after laser welding and was verified using experiments. The predicted maximum longitudinal residual stress matches measurements with an error range of 1.65% to 1.81%.\"}]","Laser Power-Dependent Microstructural Evolution and Fracture Mechanisms in Ti80 Titanium Alloy Welds | PDF",1790770768,66,[148,152,156,160],{"page_no":8,"url":149,"width":150,"height":151},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/ef951593b5d6e3fb7ffd45d2a69968f4.webp",983,1390,{"page_no":14,"url":153,"width":154,"height":155},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/d1a36fdcc1200687b66ea121b7547391.webp",982,1388,{"page_no":81,"url":157,"width":158,"height":159},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/68974104b44bda4fefb51508d18326fc.webp",981,1387,{"page_no":19,"url":161,"width":162,"height":163},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/68d4ce6c5dd46c5f585c9645b2949584.webp",980,1385]