[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-466456-105":59,"doc-detail-466456-en":130},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":123,"head_meta":125,"extra_data":127,"updated_unix":129},105,"en","influence-of-post-processing-on-s-phase-formation-during-plasma-nitriding-of-additively-manufactured-inconel-939","Influence of Post-Processing on S-Phase Formation During Plasma Nitriding of Additively Manufactured Inconel 939","","Active screen plasma nitriding (ASPN) of additively manufactured nickel-based superalloys remains insufficiently explored. This study systematically investigates ASPN on additively manufactured Inconel 939 using four post-processing routes that combine heat-treatment atmospheres (argon vs. air cooling), vibratory finishing, and lapping under identical nitriding conditions (450 °C, 8 h, 25% N2 + 75% H2, 3 hPa). The post-processing pathway strongly controls S-phase formation and mechanical response: air-cooled treatment induces a thick Al/Cr-rich oxide layer that suppresses nitrogen diffusion, yielding thin, discontinuous nitrided layers, while the inert atmosphere route avoids oxide formation and enables continuous S-phase (expanded austenite, γN) layers (~6.4 ± 0.3 µm) with high surface hardness (~1200 HV).",{"@graph":69,"@context":122},[70,84,105],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/influence-of-post-processing-on-s-phase-formation-during-plasma-nitriding-of-additively-manufactured-inconel-939/466456/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/influence-of-post-processing-on-s-phase-formation-during-plasma-nitriding-of-additively-manufactured-inconel-939/466456.png","ImageObject",300,407,{"name":92,"@type":93},"eBook King","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-10-30","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":24},"InteractionCounter",{"@type":104},"ViewAction",{"@type":106,"mainEntity":107},"FAQPage",[108,114,118],{"name":109,"@type":110,"acceptedAnswer":111},"What is the goal of the study on Inconel 939 plasma nitriding?","Question",{"text":112,"@type":113},"To evaluate how different post-processing routes affect S-phase formation during active screen plasma nitriding of additively manufactured Inconel 939.","Answer",{"name":115,"@type":110,"acceptedAnswer":116},"How do air-cooling and inert argon atmosphere post-processing differ in results?",{"text":117,"@type":113},"Air cooling promotes a thick Al/Cr-rich oxide layer that inhibits nitrogen diffusion, producing thin and discontinuous nitrided layers. The argon route avoids oxide formation and enables continuous S-phase (expanded austenite, γN) layer growth.",{"name":119,"@type":110,"acceptedAnswer":120},"Which factors are identified as controlling S-phase formation efficiency and mechanical properties?",{"text":121,"@type":113},"The study highlights the post-processing sequence—especially the heat treatment atmosphere and mechanical finishing methodology—as critical for S-phase formation and the resulting mechanical performance of nitrided layers.","https://schema.org",{"og:url":83,"og:type":124,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":126,"canonical":83},"index,follow",{"doc_id":128,"site_id":62},466456,1790812421,{"code":4,"msg":5,"data":131},{"doc_id":128,"user_id":132,"nickname":92,"user_avatar":133,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":134,"file_id":135,"file_url":136,"file_type":137,"file_size":138,"view_count":24,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":139,"language":140,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":67,"update_tm":144,"read_time":26,"preview_page_count":19,"preview_urls":145},962088006270,"https://ap-avatar.wpscdn.com/davatar_085a072bc5b1113ac321206ff7593b45","Article  \nInfluence of Post-Processing on S-Phase Formation During Plasma Nitriding of Additively Manufactured Inconel 939  \nPiotr Maj 1,*, Joanna Radziejewska 2, Ryszard Diduszko 3,4, Michał Marczak 2, Rafał Nowicki 2, Podolak-Lejtas Anna 2, Tomasz Borowski 5 and Ryszard Sitek 5  \nAcademic Editors: Damjan Klobcar, Drago Braˇcun and Tomaž Vuherer  \nReceived: 5 November 2025  \nRevised: 27 November 2025  \nAccepted: 12 December 2025  \nPublished: 30 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \n1 Faculty of Mathematical & Nature Sciences, School of Exact Sciences, Cardinal Stefan Wyszynski University, Kazimierza Wóycickiego 1/3 . 21, 01-938 Warsaw, Poland  \n2 Institute of Manufacturing Technology, Faculty of Mechanical and Industrial Technology, Warsaw University of Technology, Narbutta 85, 02-524 Warsaw, Poland; [joanna.radziejewska@pw.edu.pl](joanna.radziejewska@pw.edu.pl) (J.R.); [michal.marczak@pw.edu.pl](michal.marczak@pw.edu.pl) (M.M.); [rafal.nowicki1@pw.edu.pl](rafal.nowicki1@pw.edu.pl) (R.N.); [anna.lejtas@pw.edu.pl](anna.lejtas@pw.edu.pl) (P.-L.A.)  \n3 Polish Academy of Science, Institute of Physics, Al. Lotników 32/46, 02-668 Warsaw, Poland; [ryszard.diduszko@ncbj.gov.pl](ryszard.diduszko@ncbj.gov.pl)  \n4 National Centre for Nuclear Research, ul. Andrzeja Sołtana 7/3, 05-400 Otwock-Swierk, Poland  \n5 Faculty of Materials Science and Engineering, Warsaw University of Technology, Wołoska 141, 02-507 Warsaw, Poland; [tomasz.borowski@pw.edu.pl](tomasz.borowski@pw.edu.pl) (T.B.); [ryszard.sitek@pw.edu.pl](ryszard.sitek@pw.edu.pl) (R.S.)  \n* [Correspondence: piotr.maj@uksw.edu.pl](Correspondence: piotr.maj@uksw.edu.pl)  \nAbstract  \nActive screen plasma nitriding (ASPN) of additively manufactured nickel-based superalloys represents an understudied surface enhancement pathway. This study presents the first systematic investigation of ASPN applied to additively manufactured Inconel 939 (IN 939), evaluating four distinct post-processing routes combining heat treatment atmospheres (argon versus air cooling), vibratory finishing, and lapping under identical nitriding parameters (450 ◦ C, 8 h, 25% N2 + 75% H2, 3 hPa) . Contrasting nitriding behaviours emerged as a function of the post-processing route: the air-cooled thermal treatment (HT-air-vibr-lap) promotes formation of a thick Al/Cr-rich oxide layer (10–15 µm) that substantially inhibits nitrogen diffusion, resulting in thin and discontinuous nitrided layers. Conversely, the inert atmosphere route (HT-Ar-vibr-lap) circumvents oxide formation, enabling continuous S-phase (expanded austenite, γN) layer development of a 6.4 ± 0.3 µm thickness with exceptional surface hardness (~1200 HV, representing 3–4× enhancement relative to base material) . X-ray diffraction confirmed S-phase formation with refined lattice parameter (3 .609 Å) and secondary nitride phases (CrN-type and NbN/TaN-type precipitates) . The post-processing sequence—particularly heat treatment atmosphere and mechanical finishing methodology—emerged as a critical controlling parameter for S-phase formation efficiency and mechanical properties of nitrided layers in additively manufactured nickel-based superalloys. This work addresses a knowledge gap distinct from the existing literature on conventional Inconel systems, establishing that controlled surface modification through post-processing can achieve the required properties.  \nKeywords: Inconel 939; plasma nitriding; S-phase; expanded austenite; additive manufacturing; surface treatment  \n1. Introduction  \nAdditive manufacturing (AM), notably Laser Powder Bed Fusion (LPBF), has revolutionised the production of complex parts from high-performance alloys like Inconel 939. This nickel-based superalloy is widely used in the aerospace industry, for example, in  \nturbine blades and vanes, due to its","cbCaioea1HPlEeqz","https://ap.wps.com/l/cbCaioea1HPlEeqz","pdf",6424060,24,"English","# Introduction\n## Additive manufacturing and surface/microstructure challenges\n## Nitriding mechanism and relevance to nickel-based superalloys\n## Role of post-processing and heat treatment","[{\"question\":\"What is the goal of the study on Inconel 939 plasma nitriding?\",\"answer\":\"To evaluate how different post-processing routes affect S-phase formation during active screen plasma nitriding of additively manufactured Inconel 939.\"},{\"question\":\"How do air-cooling and inert argon atmosphere post-processing differ in results?\",\"answer\":\"Air cooling promotes a thick Al/Cr-rich oxide layer that inhibits nitrogen diffusion, producing thin and discontinuous nitrided layers. The argon route avoids oxide formation and enables continuous S-phase (expanded austenite, γN) layer growth.\"},{\"question\":\"Which factors are identified as controlling S-phase formation efficiency and mechanical properties?\",\"answer\":\"The study highlights the post-processing sequence—especially the heat treatment atmosphere and mechanical finishing methodology—as critical for S-phase formation and the resulting mechanical performance of nitrided layers.\"}]","Influence of Post-Processing on S-Phase Formation During Plasma Nitriding of Additively Manufactured Inconel 939 | PDF",1790771272,[146,150,154,158],{"page_no":8,"url":147,"width":148,"height":149},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/67f1b1778e51c50dc65d3f35cba9ea19.webp",983,1390,{"page_no":14,"url":151,"width":152,"height":153},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/84d6064ac7304d42314cf2825f7e4f7b.webp",982,1388,{"page_no":81,"url":155,"width":156,"height":157},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/899fe2b37c763ba306ff444f3a8d9397.webp",981,1387,{"page_no":19,"url":159,"width":160,"height":161},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/9578d70aaa760cbe2d727e8ad16a3c8f.webp",980,1385]