[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-462882-105":59,"doc-detail-462882-en":135},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":128,"head_meta":130,"extra_data":132,"updated_unix":134},105,"en","hygrothermal-durability-and-damage-evolution-of-bio-epoxy-based-composites-reinforced-with-different-fibre-types","Hygrothermal Durability and Damage Evolution of Bio-Epoxy-Based Composites Reinforced with Different Fibre Types","","This study investigates hygrothermal durability of bio-epoxy composites reinforced with carbon, E-glass, basalt, and flax fibres. Fibre yarns and bio-composites were exposed for 3000 h at 60 °C and 98% relative humidity. The tensile strength reduction in the fibres and the interfacial shear strength (IFSS) reduction in the composites were assessed after ageing. Chemical deterioration was evaluated using energy-dispersive X-ray spectroscopy (EDS); morphological changes were examined using a scanning electron microscope (SEM). Durability was strongly influenced by fibre type: tensile strength decreased more in carbon, glass, and basalt due to chemical degradation of sizing, while flax showed mainly physical damage. SEM and EDS indicated hydrolysis and erosion of fibre sizing and different failure mechanisms across systems, supporting reasonable performance for sustainability-driven durability-critical use.",{"@graph":69,"@context":127},[70,84,106],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/hygrothermal-durability-and-damage-evolution-of-bio-epoxy-based-composites-reinforced-with-different-fibre-types/462882/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/hygrothermal-durability-and-damage-evolution-of-bio-epoxy-based-composites-reinforced-with-different-fibre-types/462882.png","ImageObject",300,407,{"name":92,"@type":93},"Franzy","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-04","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":105},"InteractionCounter",{"@type":104},"ViewAction",13,{"@type":107,"mainEntity":108},"FAQPage",[109,115,119,123],{"name":110,"@type":111,"acceptedAnswer":112},"What environmental conditions were used for hygrothermal ageing in this study?","Question",{"text":113,"@type":114},"Fibre yarns and bio-composites were exposed for 3000 h at 60 °C and 98% relative humidity.","Answer",{"name":116,"@type":111,"acceptedAnswer":117},"Which material property reductions were evaluated after ageing?",{"text":118,"@type":114},"The study assessed tensile strength reduction in the fibres and interfacial shear strength (IFSS) reduction in the composites.",{"name":120,"@type":111,"acceptedAnswer":121},"How did fibre type affect durability results?",{"text":122,"@type":114},"Durability was significantly influenced by fibre type: tensile strength reduction was higher for carbon, glass, and basalt than for flax, and IFSS reduction was highest in flax (10%) and lowest in carbon (4%).",{"name":124,"@type":111,"acceptedAnswer":125},"What failure and degradation mechanisms were identified?",{"text":126,"@type":114},"EDS indicated hydrolysis and erosion of fibre sizing, while SEM showed matrix-dominated failure in carbon/bio-epoxy, interfacial debonding in glass and basalt composites, and fibre slip and pull-out in flax/bio-epoxy.","https://schema.org",{"og:url":83,"og:type":129,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":131,"canonical":83},"index,follow",{"doc_id":133,"site_id":62},462882,1791158505,{"code":4,"msg":5,"data":136},{"doc_id":133,"user_id":137,"nickname":92,"user_avatar":138,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":139,"file_id":140,"file_url":141,"file_type":142,"file_size":143,"view_count":105,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":46,"language":144,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":145,"faqs":146,"seo_title":147,"seo_description":67,"update_tm":148,"read_time":31,"preview_page_count":19,"preview_urls":149},2336478945519,"https://ap-avatar.wpscdn.com/davatar_085a072bc5b1113ac321206ff7593b45","Article  \nHygrothermal Durability and Damage Evolution of Bio-Epoxy-Based Composites Reinforced with Different Fibre Types  \nAbdullah Iftikhar 1, Allan Manalo 1,*, Zaneta Senselova 1, Wahid Ferdous 1, Mazhar Peerzada 1, Hannah Seligmann 1, Kate Nguyen 2 and Brahim Benmokrane 3  \nAcademic Editors: Diego Vergara and Antonio Del Bosque  \nReceived: 5 December 2025  \nRevised: 19 December 2025  \nAccepted: 22 December 2025  \nPublished: 25 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \n1 Centre for Future Materials, University of Southern Queensland, Toowoomba, QLD 4350, Australia; [abdullah.iftikhar@unisq.edu.au](abdullah.iftikhar@unisq.edu.au) (A.I.); [zaneta.senselova@unisq.edu.au](zaneta.senselova@unisq.edu.au) (Z.S.); [wahid.ferdous@unisq.edu.au](wahid.ferdous@unisq.edu.au) (W.F.); [mazhar.peerzada@unisq.edu.au](mazhar.peerzada@unisq.edu.au) (M.P.); [hannah.seligmann@unisq.edu.au](hannah.seligmann@unisq.edu.au) (H.S.)  \n2 School of Engineering, RMIT University, GPO Box 2476, Melbourne, VIC 3001, Australia; [kate.nguyen@rmit.edu.au](kate.nguyen@rmit.edu.au)  \n3 Department of Civil and Building Engineering, University of Sherbrooke, Sherbrooke, QC J1K 2R1, Canada; [brahim.benmokrane@usherbrooke.ca](brahim.benmokrane@usherbrooke.ca)  \n* Correspondence: [allan.manalo@unisq.edu.au](allan.manalo@unisq.edu.au)  \nAbstract  \nThis study investigates hygrothermal durability of bio-epoxy composites reinforced with carbon, E-glass, basalt, and flax fibres. Fibre yarns and bio-composites were exposed for 3000 h at 60 ◦ C and 98% relative humidity. The tensile strength reduction in the fibres and the interfacial shear strength (IFSS) reduction in the composites were assessed after ageing. Chemical deterioration was evaluated using energy-dispersive X-ray spectroscopy (EDS); morphological changes in fibres and composites fracture surfaces were examined using a scanning electron microscope (SEM) . Results indicated that the durability was significantly influenced by fibre types. Tensile strength reduction was higher in carbon, glass and basalt compared to flax yarns because of chemical degradation of the sizing layer in synthetic fibres, while only physical damage was observed in flax. The IFSS reduction was highest in flax composites (10%), and lowest in carbon (4%) . EDS indicated the hydrolysis and erosion of fibre sizing, with reduced silica content in glass and basalt fibres. SEM revealed matrix-dominated failure in carbon/bio-epoxy, interfacial debonding in glass and basalt composites, fibre slip and pull-out in flax/bio-epoxy. Overall, the results highlighted damage propagation pathways and demonstrated that bio-epoxy composites exhibited reasonable performance under hygrothermal ageing, supporting their potential as a sustainable alternative in durability-critical applications.  \nKeywords: hygrothermal durability; material degradation; bio-composites; bio-based polymers; environmental ageing; fracture behaviour  \n1. Introduction  \nInterest in the use of fibre-reinforced polymer (FRP) composites has increased because of their corrosion resistance, light weight, high strength-to-weight ratio, and high stiffness-to-weight ratio [1,2] . In civil engineering applications, FRP composites are now commonly used in bridge decks, railway sleepers, building facades, marine structures, wind turbine blades, and electrical transmission lines [3–7] . Various synthetic and natural fibres are used to manufacture FRP composites, depending on the intended use during  \nservice life. Synthetic fibres are preferred for highly demanding structural applications. For instance, glass fibres are used for all composite civil infrastructure and carbon fibres are preferred when the strength requirements are even higher [8] . Basalt fibres have also emerged as a competitive substitute for glass fi","cbCaid0qDjeYcWGM","https://ap.wps.com/l/cbCaid0qDjeYcWGM","pdf",20547851,"English","# Abstract\n# Keywords\n# 1. Introduction","[{\"question\":\"What environmental conditions were used for hygrothermal ageing in this study?\",\"answer\":\"Fibre yarns and bio-composites were exposed for 3000 h at 60 °C and 98% relative humidity.\"},{\"question\":\"Which material property reductions were evaluated after ageing?\",\"answer\":\"The study assessed tensile strength reduction in the fibres and interfacial shear strength (IFSS) reduction in the composites.\"},{\"question\":\"How did fibre type affect durability results?\",\"answer\":\"Durability was significantly influenced by fibre type: tensile strength reduction was higher for carbon, glass, and basalt than for flax, and IFSS reduction was highest in flax (10%) and lowest in carbon (4%).\"},{\"question\":\"What failure and degradation mechanisms were identified?\",\"answer\":\"EDS indicated hydrolysis and erosion of fibre sizing, while SEM showed matrix-dominated failure in carbon/bio-epoxy, interfacial debonding in glass and basalt composites, and fibre slip and pull-out in flax/bio-epoxy.\"}]","Hygrothermal Durability and Damage Evolution of Bio-Epoxy-Based Composites Reinforced with Different Fibre Types | PDF",1790765625,[150,154,158,162],{"page_no":8,"url":151,"width":152,"height":153},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/bc25d4546431d7eca2e489dfc3a4f683.webp",983,1390,{"page_no":14,"url":155,"width":156,"height":157},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/14a207da195582947589dc92a380245a.webp",982,1388,{"page_no":81,"url":159,"width":160,"height":161},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/98630e5c85a87a032eca852d0bca0fda.webp",981,1387,{"page_no":19,"url":163,"width":164,"height":165},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/01ed268afd9e60ae010647f17495d053.webp",980,1385]