[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-466262-105":59,"doc-detail-466262-en":130},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":123,"head_meta":125,"extra_data":127,"updated_unix":129},105,"en","hot-deformation-behavior-and-microstructure-evolution-of-a-fe-ni-cr-based-superalloy","Hot Deformation Behavior and Microstructure Evolution of a Fe-Ni-Cr Based Superalloy","","The present study systematically investigated the hot deformation behavior of GH2787 superalloy within the temperature range of 1060–1120 °C and strain rates of 0.1–10 s−1. An Arrhenius-type constitutive equation was developed that accurately predicts the flow behavior, and the calculated thermal deformation activation energy Q is 364,401.19 J/mol. The hot working map identified two preferred processing regions with power dissipation efficiency exceeding 0.3, with no flow instability observed. Microstructural evolution is governed by DDRX as the dominant mechanism, aided by CDRX synergy, providing foundations for optimizing hot working processes.",{"@graph":69,"@context":122},[70,84,105],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/hot-deformation-behavior-and-microstructure-evolution-of-a-fe-ni-cr-based-superalloy/466262/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/hot-deformation-behavior-and-microstructure-evolution-of-a-fe-ni-cr-based-superalloy/466262.png","ImageObject",300,407,{"name":92,"@type":93},"Cart","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-10-31","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":52},"InteractionCounter",{"@type":104},"ViewAction",{"@type":106,"mainEntity":107},"FAQPage",[108,114,118],{"name":109,"@type":110,"acceptedAnswer":111},"What temperature and strain-rate range was used to study GH2787 hot deformation?","Question",{"text":112,"@type":113},"The study investigated GH2787 within 1060–1120 °C and strain rates of 0.1–10 s−1.","Answer",{"name":115,"@type":110,"acceptedAnswer":116},"What model was developed to predict the flow behavior of the superalloy?",{"text":117,"@type":113},"An Arrhenius-type constitutive equation was developed to predict flow behavior, and it yielded a thermal deformation activation energy Q of 364,401.19 J/mol.",{"name":119,"@type":110,"acceptedAnswer":120},"Which dynamic recrystallization mechanisms govern microstructure evolution in GH2787?",{"text":121,"@type":113},"Discontinuous dynamic recrystallization (via grain boundary bulging nucleation) is dominant, while continuous dynamic recrystallization (via subgrain rotation and coalescence) acts as a synergistic auxiliary mechanism.","https://schema.org",{"og:url":83,"og:type":124,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":126,"canonical":83},"index,follow",{"doc_id":128,"site_id":62},466262,1790820633,{"code":4,"msg":5,"data":131},{"doc_id":128,"user_id":132,"nickname":92,"user_avatar":133,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":134,"file_id":135,"file_url":136,"file_type":137,"file_size":138,"view_count":52,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":139,"language":140,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":67,"update_tm":144,"read_time":145,"preview_page_count":19,"preview_urls":146},18829141979164,"https://eur-avatar.wpscdn.com/davatar_6f874abed73319feea01a86fa6f0fab8","Article  \nHot Deformation Behavior and Microstructure Evolution of a Fe-Ni-Cr Based Superalloy  \nYan Wang 1,2,3, Tianyi Wang 4, Guohua Xu 4, Shengkai Gong 1, Ning Liu 5, Shusuo Li 1, Qiuyu Wang 2, Wenqi Guo 1, * and Biao Zhang 4,6, *  \nReceived: 17 November 2025  \nRevised: 18 December 2025  \nAccepted: 19 December 2025  \nPublished: 23 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \n1 Research Institute of Aero-Engine, Beihang University, Beijing 100191, China; [wangyan20251120@163.com](wangyan20251120@163.com) (Y.W.)  \n2 AECC Chengdu Engine Co., Ltd., Chengdu 610503, China  \n3 Taihang Laboratory, Chengdu 610213, China  \n4 Gaona Aero Material Co., Ltd., Beijing 100081, China  \n5 Fushun Special Steel Co., Ltd., Fushun 113001, China  \n6 School of Materials Science and Engineering, University of Science and Technology Beijing, Beijing 100083, China  \n* Correspondence: [guowenqi@buaa.edu.cn](guowenqi@buaa.edu.cn) (W.G.); [biaozhang0525@163.com](biaozhang0525@163.com) (B.Z.)  \nAbstract  \nThe present study systematically investigated the hot deformation behavior of GH2787 superalloy within the temperature range of 1060–1120 ◦ C and strain rates of 0.1–10 s−1 . An Arrhenius-type constitutive equation was developed that accurately predicts the flow behavior, and the calculated thermal deformation activation energy Q is 364,401.19 J/mol. The hot working map was constructed based on the dynamic material model, which identified two preferred processing regions with power dissipation efficiency exceeding 0.3, and no flow instability was observed across the entire parameter range. Microstructural analysis reveals that the extent of dynamic recrystallization significantly increases with rising temperature and strain rate. Discontinuous dynamic recrystallization (via grain boundary bulging nucleation) serves as the dominant recrystallization mechanism in GH2787 superalloy during hot deformation, while continuous dynamic recrystallization (via subgrain rotation and coalescence) acts as a synergistic auxiliary mechanism, jointly driving microstructural evolution. This study provides important theoretical foundations for optimizing the hot working processes of GH2787 superalloy.  \nKeywords: GH2787 superalloy; hot deformation; microstructural evolution; DRX mechanism; processing maps  \n1. Introduction  \nNi-based superalloys serve as cornerstone materials for high-temperature critical components in the aerospace and energy industries, particularly for turbine disks, blades, and other essential parts. Their exceptional mechanical strength, outstanding creep resistance, and remarkable microstructural stability under extreme thermomechanical loads are vital for ensuring the efficiency, reliability, and safety of advanced engines [1–3] . Among these superalloys, GH2787 superalloy is widely utilized for high-temperature components such as turbine engine working blades operating at 700–800 ◦ C and compressor blades serving at 500–700 ◦ C, owing to its high strength coupled with good ductility, excellent fatigue resistance, and superior corrosion performance [4,5] . The in-service performance of these critical components is intrinsically linked to the microstructure developed during hotforming processes like forging, rolling, or extrusion. These thermomechanical processing  \nroutes involve complex deformation under controlled temperatures and strain rates. The hot deformation behavior of superalloys is characterized by a series of competing metallurgical phenomena, including work hardening, dynamic recovery (DRV), and dynamic recrystallization (DRX) [6–9] . The interplay of these mechanisms dictates the evolution of grain size, phase distribution, and dislocation substructures, ultimately determining the final mechanical properties of the forged components. Consequently, a comprehensi","cbCaio6LIbXpbm9v","https://ap.wps.com/l/cbCaio6LIbXpbm9v","pdf",5838655,14,"English","# Abstract\n# Keywords\n# 1. Introduction","[{\"question\":\"What temperature and strain-rate range was used to study GH2787 hot deformation?\",\"answer\":\"The study investigated GH2787 within 1060–1120 °C and strain rates of 0.1–10 s−1.\"},{\"question\":\"What model was developed to predict the flow behavior of the superalloy?\",\"answer\":\"An Arrhenius-type constitutive equation was developed to predict flow behavior, and it yielded a thermal deformation activation energy Q of 364,401.19 J/mol.\"},{\"question\":\"Which dynamic recrystallization mechanisms govern microstructure evolution in GH2787?\",\"answer\":\"Discontinuous dynamic recrystallization (via grain boundary bulging nucleation) is dominant, while continuous dynamic recrystallization (via subgrain rotation and coalescence) acts as a synergistic auxiliary mechanism.\"}]","Hot Deformation Behavior and Microstructure Evolution of a Fe-Ni-Cr Based Superalloy | PDF",1790770915,35,[147,151,155,159],{"page_no":8,"url":148,"width":149,"height":150},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/abef4809f67496f8bd9567fe3bee4006.webp",983,1390,{"page_no":14,"url":152,"width":153,"height":154},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/ac224654ba9959861211d60348204976.webp",982,1388,{"page_no":81,"url":156,"width":157,"height":158},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/5f8937fc6a3137c1ceb64c5c555cf61b.webp",981,1387,{"page_no":19,"url":160,"width":161,"height":162},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/5bf766c2d8da8b88f524a482880df709.webp",980,1385]