[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-466285-105":59,"doc-detail-466285-en":130},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":123,"head_meta":125,"extra_data":127,"updated_unix":129},105,"en","high-temperature-deformation-behavior-of-powder-metallurgy-ti-4zr-6al-06si-05mo-alloy","High-Temperature Deformation Behavior of Powder Metallurgy Ti-4Zr-6Al-0.6Si-0.5Mo Alloy","","Hot deformation behavior of the powder metallurgy Ti-4Zr-6Al-0.6Si-0.5Mo high-temperature titanium alloy was investigated across 800–1100 °C, strain rates of 0.001–1 s−1, and true strain of 0.5. Flow stress curves at different deformation conditions were analyzed to derive a constitutive equation linking flow stress, deformation temperature, and strain rate. Processing maps based on instability evaluation were used to identify safe and instability domains, determining the optimal hot-processing window and deformation-failure regions.",{"@graph":69,"@context":122},[70,84,105],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/high-temperature-deformation-behavior-of-powder-metallurgy-ti-4zr-6al-06si-05mo-alloy/466285/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/high-temperature-deformation-behavior-of-powder-metallurgy-ti-4zr-6al-06si-05mo-alloy/466285.png","ImageObject",300,407,{"name":92,"@type":93},"Adam","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-10-30","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":44},"InteractionCounter",{"@type":104},"ViewAction",{"@type":106,"mainEntity":107},"FAQPage",[108,114,118],{"name":109,"@type":110,"acceptedAnswer":111},"Which deformation parameters were used to study the alloy’s hot deformation behavior?","Question",{"text":112,"@type":113},"The study investigated temperatures from 800–1100 °C, strain rates from 0.001–1 s−1, and a true strain of 0.5.","Answer",{"name":115,"@type":110,"acceptedAnswer":116},"What analytical method was used to relate flow stress to deformation conditions?",{"text":117,"@type":113},"Flow stress curves were analyzed and a constitutive equation was established to describe the correlation among flow stress, deformation temperature, and strain rate.",{"name":119,"@type":110,"acceptedAnswer":120},"How were instability domains and the optimal hot processing window determined?",{"text":121,"@type":113},"Processing maps were employed to identify instability domains and the optimal hot-processing window for the alloy.","https://schema.org",{"og:url":83,"og:type":124,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":126,"canonical":83},"index,follow",{"doc_id":128,"site_id":62},466285,1790812629,{"code":4,"msg":5,"data":131},{"doc_id":128,"user_id":132,"nickname":92,"user_avatar":133,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":134,"file_id":135,"file_url":136,"file_type":137,"file_size":138,"view_count":44,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":139,"language":140,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":67,"update_tm":144,"read_time":41,"preview_page_count":19,"preview_urls":145},1374404737137,"https://ap-avatar.wpscdn.com/davatar_155a257f0dc6eb9ab79c44ca47cae57d","Article  \nHigh-Temperature Deformation Behavior of Powder Metallurgy Ti-4Zr-6Al-0.6Si-0.5Mo Alloy  \nZongshu Li 1, Wentao Liu 1,2, Jian Wang 2, Yuankui Cao 2, Qihong Fang 3, Ao Fu 2,* and Bin Liu 2  \nAcademic Editor: Andrey Belyakov  \nReceived: 27 November 2025  \nRevised: 17 December 2025  \nAccepted: 26 December 2025  \nPublished: 29 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \n1 China North Nuclear Fuel Co., Ltd., Baotou 014035, China; [lizongshu0909@163.com](lizongshu0909@163.com) (Z.L.); [liuwentao0506@163.com](liuwentao0506@163.com) (W.L.)  \n2 State Key Laboratory of Powder Metallurgy, Central South University, Changsha 410083, China; [213307006@csu.edu.cn](213307006@csu.edu.cn) (J.W.); [caoyuankui@csu.edu.cn](caoyuankui@csu.edu.cn) (Y.C.); [binliu@csu.edu.cn](binliu@csu.edu.cn) (B.L.)  \n3 State Key Laboratory of Advanced Design and Manufacturing Technology for Vehicle, College of Mechanical and Vehicle Engineering, Hunan University, Changsha 410082, China; [fangqh1327@hnu.edu.cn](fangqh1327@hnu.edu.cn)  \n* Correspondence: [aofu_ice@csu.edu.cn](aofu_ice@csu.edu.cn)  \nAbstract  \nThe hot deformation behavior of Ti-4Zr-6Al-0.6Si-0.5Mo high-temperature titanium alloy was investigated under temperatures of 800–1100 ◦ C, strain rates of 0.001–1 s−1, and a true strain of 0.5 . Flow stress curves under different temperatures and strain rates were analyzed, and a constitutive equation that depicts the correlation among flow stress, deformation temperature, and strain rate was established. Processing maps were employed for determining the instability domains as well as optimal hot processing window. The results show that the optimal hot processing window for the alloy is a deformation temperature of 950–1100◦ C and a strain rate of 0.001–0.01 s−1 . Flow instability occurred within two domains: 800–850◦ C at strain rates of 0 . 1–1 s −1 and 900–1075◦ C at strain rates of 0 .01–0. 1 s −1, where the alloy is prone to cracking, resulting in processing failure.  \nKeywords: titanium alloy; high-temperature deformation; constitutive equation; processing map  \n1. Introduction  \nNear-α high-temperature titanium alloys represent a prominent development trend within the realm of titanium alloys over the past decade, which synergistically combine low density with high strength, enabling structural weight reduction while preserving loadbearing stability [1–4] . Furthermore, they exhibit reliable high-temperature mechanical properties, rendering them adaptable to complex and demanding service conditions [5–8] . As a result, they have been widely adopted in critical industries—including aerospace, shipbuilding, and the chemical industry—providing a robust material basis for the development of lightweight, high-performance equipment and underscoring their significant application value and development potential [9–12] .  \nHot working is an essential process in manufacturing metal components, which not only imparts the desired shape and dimensions but also further enhances the overall properties of the alloy [13–15] . Compared with steels and aluminum alloys, titanium alloys are often more difficult to hot work due to their unique crystal structure [16,17] . During hot working, deformation temperature and strain rate represent the two most vital parameters, requiring precise control to ensure uniform deformation [15,18,19] . Thermomechanical simulation experiments are capable of efficiently simulating the deformation characteristics under various temperatures and strain rates, reproducing the material’s response during  \nactual hot working [20,21] . Processing maps founded on the dynamic materials model (DMM) are employed to evaluate and predict material workability, visually delineating the safe and instability domains [22–24] . However, investigations into the microstructural ","cbCaihox4r10X0Oh","https://ap.wps.com/l/cbCaihox4r10X0Oh","pdf",4008214,12,"English","# Abstract\n# Introduction\n# Experimental Procedure","[{\"question\":\"Which deformation parameters were used to study the alloy’s hot deformation behavior?\",\"answer\":\"The study investigated temperatures from 800–1100 °C, strain rates from 0.001–1 s−1, and a true strain of 0.5.\"},{\"question\":\"What analytical method was used to relate flow stress to deformation conditions?\",\"answer\":\"Flow stress curves were analyzed and a constitutive equation was established to describe the correlation among flow stress, deformation temperature, and strain rate.\"},{\"question\":\"How were instability domains and the optimal hot processing window determined?\",\"answer\":\"Processing maps were employed to identify instability domains and the optimal hot-processing window for the alloy.\"}]","High-Temperature Deformation Behavior of Powder Metallurgy Ti-4Zr-6Al-0.6Si-0.5Mo Alloy | PDF",1790771011,[146,150,154,158],{"page_no":8,"url":147,"width":148,"height":149},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/8a6794e9780ed4bc4ea877d36acebaf4.webp",983,1390,{"page_no":14,"url":151,"width":152,"height":153},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/f24738ef9e0e8b4f4617b0f1aacaceb4.webp",982,1388,{"page_no":81,"url":155,"width":156,"height":157},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/64a0b7f0cc1a4884ad791a8c9e71828f.webp",981,1387,{"page_no":19,"url":159,"width":160,"height":161},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/29e22c0085d259d67e28e8686b5fad58.webp",980,1385]