[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-466611-105":59,"doc-detail-466611-en":131},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":124,"head_meta":126,"extra_data":128,"updated_unix":130},105,"en","evolution-of-the-metallographic-structure-of-additively-manufactured-ti-6al-4v-and-ti-6al-7nb-titanium-alloys","Evolution of the Metallographic Structure of Additively Manufactured Ti-6Al-4V and Ti-6Al-7Nb Titanium Alloys","","The study evaluates structural changes and their effects on functional properties of Ti-6Al-4V and Ti-6Al-7Nb titanium alloys produced by L-PBF. In the as-built state, high strength from metastable α’ martensite coexists with limited ductility. Heat treatment at 850–1000 °C for 1 h, followed by aging at 500 °C for 4 h under argon, drives a gradual transformation from L-PBF columnar structure to equilibrium Widmanstätten morphology. Decomposition of martensite and formation of an α + β mixture alter microhardness and mechanical behavior, with hardness reductions and improved elongation, especially for Ti-6Al-7Nb.",{"@graph":69,"@context":123},[70,84,106],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/evolution-of-the-metallographic-structure-of-additively-manufactured-ti-6al-4v-and-ti-6al-7nb-titanium-alloys/466611/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/evolution-of-the-metallographic-structure-of-additively-manufactured-ti-6al-4v-and-ti-6al-7nb-titanium-alloys/466611.png","ImageObject",300,407,{"name":92,"@type":93},"Grenda","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-14","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":105},"InteractionCounter",{"@type":104},"ViewAction",11,{"@type":107,"mainEntity":108},"FAQPage",[109,115,119],{"name":110,"@type":111,"acceptedAnswer":112},"What alloys and manufacturing method are investigated?","Question",{"text":113,"@type":114},"The study focuses on Ti-6Al-4V and Ti-6Al-7Nb titanium alloys produced by laser powder bed fusion (L-PBF).","Answer",{"name":116,"@type":111,"acceptedAnswer":117},"How does the study modify the samples after fabrication?",{"text":118,"@type":114},"Samples are heat treated at 850–1000 °C for 1 hour, then aged at 500 °C for 4 hours in an argon atmosphere.",{"name":120,"@type":111,"acceptedAnswer":121},"What microstructural change is observed after heat treatment?",{"text":122,"@type":114},"The microstructure gradually transforms from the L-PBF columnar structure to an equilibrium Widmanstätten microstructure via martensite decomposition and formation of an α + β phase mixture.","https://schema.org",{"og:url":83,"og:type":125,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":127,"canonical":83},"index,follow",{"doc_id":129,"site_id":62},466611,1790804260,{"code":4,"msg":5,"data":132},{"doc_id":129,"user_id":133,"nickname":92,"user_avatar":134,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":135,"file_id":136,"file_url":137,"file_type":138,"file_size":139,"view_count":105,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":140,"language":141,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":142,"faqs":143,"seo_title":144,"seo_description":67,"update_tm":145,"read_time":146,"preview_page_count":19,"preview_urls":147},7971474921005,"https://ap-avatar.wpscdn.com/davatar_29158cc5080c5b710cf443261637dec0","Article  \nEvolution of the Metallographic Structure of Additively Manufactured Ti-6Al-4V and Ti-6Al-7Nb Titanium Alloys Dorota Laskowska *, Błaej Bałasz * and Łukasz Z˙urawski   \nAcademic Editor: Wei Guo  \nReceived: 4 December 2025  \nRevised: 18 December 2025  \nAccepted: 22 December 2025  \nPublished: 25 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \nFaculty of Mechanical Engineering and Energy, Koszalin University of Technology, ´Sniadeckich 2, 75-453 Koszalin, Poland; [lukasz.zurawski@tu.koszalin.pl](lukasz.zurawski@tu.koszalin.pl)  \n* Correspondence: [dorota.laskowska@tu.koszalin.pl](dorota.laskowska@tu.koszalin.pl) (D.L.); [blazej.balasz@tu.koszalin.pl](blazej.balasz@tu.koszalin.pl) (B.B.)  \nAbstract  \nThe aim of this study was to evaluate structural changes and their impact on the functional properties of Ti-6Al-4V and Ti-6Al-7Nb titanium alloys produced by L-PBF. In the as-built condition, these alloys, despite high strength due to the presence of metastable α’ martensite, exhibit limited ductility. The samples were subjected to heat treatment at 850–1000 ◦ C for 1 h, followed by aging at 500 ◦ C for 4 h in an argon atmosphere. Analysis revealed a gradual microstructural transformation from the columnar structure characteristic of L-PBF to an equilibrium Widmanstätten microstructure. As a result of the decomposition of martensite and the formation of an α + β phase mixture, changes in microhardness and mechanical properties were observed. After heat treatment, the microhardness decreased by 15% for Ti-6Al-4V (from 427 ± 1 HV to 362 ± 25 HV) and by 12% for Ti-6Al-7Nb (from 408 ± 6 HV to 359 ± 15 HV) . The Ti-6Al-7Nb alloy exhibited higher maximum elongation (7.7 ± 1.1%)  \nthan Ti-6Al-4V (4.8 ± 0.5%) due to a greater fraction of the β phase. The results highlight the critical role of the controlled α′ →α + β transformation in tailoring the properties of titanium alloys and provide a basis for optimizing manufacturing processes for medical and aerospace components.  \nKeywords: additive manufacturing; titan-base alloys; heat treatment; microstructural transformation; mechanical properties  \n1. Introduction  \nTitanium and its alloys are extensively utilized in dental medicine, orthopedics, and implantology due to their exceptional corrosion resistance, highly specific mechanical properties, and biocompatibility. In response to the growing demand for components with highly customized geometries and tailored properties, additive manufacturing technologies—particularly laser powder bed fusion (L-PBF)—have experienced significant advancements in recent years. L-PBF operates by selectively melting a powder bed in accordance with a CAD model using a high-energy laser. Comprehensive details regarding the technology are provided in [1–3] .  \nAmong titanium alloys, Ti-6Al-4V is the most commonly employed in medical applications. However, it is anticipated that non-vanadium alloys may see wider application due to the reported cytotoxicity of vanadium ions [4,5] . Studies conducted by Costa et al. [6] demonstrated that the continuous exposition for V ions and their accumulation in surrounding tissues can induce cytotoxic effects, raising concerns regarding long-term biocompatibility—particularly for implants susceptible to corrosion or wear. Furthermore,  \nresearch has shown that Ti-6Al-7Nb exhibits superior corrosion resistance compared to Ti- 6Al-4V [7,8]. Both alloys are α + β dual-phase alloys, in which aluminum acts as the α-phase stabilizer, while vanadium and niobium serve as the β-phase stabilizers, respectively [9] .  \nSeveral factors influence the properties of titanium alloys, among which microstructure is one of the most significant. It is primarily governed by the alloy’s chemical composition and the manufacturing process. The specific characteristics o","cbCaidnP6H7pCwpr","https://ap.wps.com/l/cbCaidnP6H7pCwpr","pdf",8360032,17,"English","# 1. Introduction\n## Titanium alloys in biomedical applications and implant biocompatibility\n## Role of additive manufacturing (L-PBF) and resulting microstructure\n## Influence of composition and ISO 5832-3:2021 elongation targets\n## Heat treatment as a tool to tailor microstructure and properties","[{\"question\":\"What alloys and manufacturing method are investigated?\",\"answer\":\"The study focuses on Ti-6Al-4V and Ti-6Al-7Nb titanium alloys produced by laser powder bed fusion (L-PBF).\"},{\"question\":\"How does the study modify the samples after fabrication?\",\"answer\":\"Samples are heat treated at 850–1000 °C for 1 hour, then aged at 500 °C for 4 hours in an argon atmosphere.\"},{\"question\":\"What microstructural change is observed after heat treatment?\",\"answer\":\"The microstructure gradually transforms from the L-PBF columnar structure to an equilibrium Widmanstätten microstructure via martensite decomposition and formation of an α + β phase mixture.\"}]","Evolution of the Metallographic Structure of Additively Manufactured Ti-6Al-4V and Ti-6Al-7Nb Titanium Alloys | PDF",1790771580,43,[148,152,156,160],{"page_no":8,"url":149,"width":150,"height":151},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/c01c9dd7325e4ca351ac6048d4b10c2d.webp",983,1390,{"page_no":14,"url":153,"width":154,"height":155},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/96a2c8e7804cdaa9fe0f78f321f74f67.webp",982,1388,{"page_no":81,"url":157,"width":158,"height":159},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/c43a1966c99f586cdc59082a03c541d0.webp",981,1387,{"page_no":19,"url":161,"width":162,"height":163},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/0c85c4bb58cbb2120391d023ddfc616a.webp",980,1385]