[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-463217-105":59,"doc-detail-463217-en":130},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":123,"head_meta":125,"extra_data":127,"updated_unix":129},105,"en","evaluation-of-the-seismic-behavior-of-carbon-grid-reinforced-walls-with-varying-anchorage-and-axial-load-ratios","Evaluation of the Seismic Behavior of Carbon-Grid-Reinforced Walls with Varying Anchorage and Axial Load Ratios","","Fiber-reinforced polymers (FRPs) are increasingly used to replace steel rebar in concrete. This study evaluates the seismic performance of concrete walls reinforced with grid-type carbon FRP (CFRP) using quasi-static cyclic loading and compares results with reinforced concrete (RC) walls. Variables include the anchorage length ratio (foundation to wall) and the axial force ratio. The equivalent stiffness to compression-edge cover concrete crushing averages 0.14, indicating stiffness degradation after cracking. Carbon-grid specimens show bilinear skeleton behavior with failure governed by compression-edge crushing, and energy absorption trends under story drift.",{"@graph":69,"@context":122},[70,84,105],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/evaluation-of-the-seismic-behavior-of-carbon-grid-reinforced-walls-with-varying-anchorage-and-axial-load-ratios/463217/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/evaluation-of-the-seismic-behavior-of-carbon-grid-reinforced-walls-with-varying-anchorage-and-axial-load-ratios/463217.png","ImageObject",300,407,{"name":92,"@type":93},"Rainbow Cat","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-03","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":52},"InteractionCounter",{"@type":104},"ViewAction",{"@type":106,"mainEntity":107},"FAQPage",[108,114,118],{"name":109,"@type":110,"acceptedAnswer":111},"What reinforcement system is evaluated in this study?","Question",{"text":112,"@type":113},"The study evaluates concrete walls reinforced with grid-type carbon FRP (CFRP), also comparing their response with reinforced concrete (RC) walls.","Answer",{"name":115,"@type":110,"acceptedAnswer":116},"Which experimental variables control the behavior of the carbon-grid reinforced walls?",{"text":117,"@type":113},"The variables are the ratio of the carbon-grid anchorage length in the foundation to the wall length, and the axial force ratio.",{"name":119,"@type":110,"acceptedAnswer":120},"How does anchorage length ratio and axial force ratio affect the crushing-load level?",{"text":121,"@type":113},"The load at compression-edge cover concrete crushing increases by 1.10 times with increasing axial force ratio and decreases by 0.96 times as the anchorage length ratio decreases.","https://schema.org",{"og:url":83,"og:type":124,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":126,"canonical":83},"index,follow",{"doc_id":128,"site_id":62},463217,1790895375,{"code":4,"msg":5,"data":131},{"doc_id":128,"user_id":132,"nickname":92,"user_avatar":133,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":134,"file_id":135,"file_url":136,"file_type":137,"file_size":138,"view_count":52,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":139,"language":140,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":67,"update_tm":144,"read_time":145,"preview_page_count":19,"preview_urls":146},962090769181,"https://ap-avatar.wpscdn.com/davatar_6f874abed73319feea01a86fa6f0fab8","Article  \nEvaluation of the Seismic Behavior of Carbon-Grid-Reinforced Walls with Varying Anchorage and Axial Load Ratios  \nKyung-Min Kim 1,*, Sung-Woo Park 1, Bhum-Keun Song 2, Kyung-Jae Min 2 and Seon-Hee Yoon 3  \nAcademic Editor: Zhanhua Wang  \nReceived: 11 December 2025  \nRevised: 27 December 2025  \nAccepted: 30 December 2025  \nPublished: 5 January 2026  \nCopyright: © 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \n1 Seismic Safety Center, Korea Conformity Laboratories (KCL), Suwon 16229, Republic of Korea; [sungwoo@kcl.re.kr](sungwoo@kcl.re.kr)  \n2 Korea Carbon Industry Promotion Agency, Jeonju 54853, Republic of Korea; [bksong@kcarbon.or.kr](bksong@kcarbon.or.kr) (B.-K.S.); [bluemy@kcarbon.or.kr](bluemy@kcarbon.or.kr) (K.-J.M.)  \n3 High In Tech Co., Ltd., Ulsan 44785, Republic of Korea; [w470470@nate.com](w470470@nate.com)  \n* Correspondence: [kymkim@kcl.re.kr](kymkim@kcl.re.kr)  \nAbstract  \nFiber-reinforced polymers (FRPs) are being increasingly used to replace rebars as reinforcements for concrete. This study evaluated the seismic behavior of concrete walls reinforced with grid-type carbon FRP (CFRP; carbon grid) through quasi-static cyclic tests and compared the results with that of the reinforced concrete (RC) wall. The experimental variables were the ratio of the carbon-grid anchorage length in the foundation to the wall length and the axial force ratio. Based on the results of the quasi-static cyclic tests, the ratio of the equivalent stiffness at the crushing of the compression-edge cover concrete to the initial stiffness of the carbon-grid-reinforced concrete specimens was 0.14 on average. This indicates that the specimens reached their maximum load due to the crushing of the compression-edge cover concrete after a significant reduction in stiffness due to cracking. The skeleton curve for the carbon-grid-reinforced concrete specimens was found to be bilinear, with reduced stiffness due to cracking and failure due to the crushing of the compression-edge cover concrete, making it definable and predictable. Additionally, in specimens with a high axial force or small ratio of the anchorage length in the foundation to the wall length, some of the longitudinal CFRP strands fractured at the same time as they reached the failure load. Moreover, the load at the crushing of the compression-edge cover concrete of the carbon-grid-reinforced concrete specimen increased by 1.10 times with the increase in the axial force ratio and decreased by 0.96 times with the decrease in the ratio of the anchorage length in the foundation to the wall length. It was found to be 0.73–0.80 times the flexural strength based on the assumption of plane sections remaining plane. In comparison with RC specimen, the cumulative absorbed energy of the carbon-grid-reinforced concrete specimen began to decrease after a story drift ratio of 1%, and the cumulative absorbed energy up to the target story drift ratio of 3.0% was found to be 0.60–0.62 times that of the RC specimen.  \nKeywords: reinforced concrete; fiber-reinforced polymer; grid-type carbon-fiber-reinforced polymer reinforcement; carbon-grid-reinforced concrete; seismic behavior  \n1. Introduction  \nReinforced concrete (RC) structures can experience damage such as superficial cracking when exposed to marine environments, allowing chloride ions to penetrate inside the members. This can lead to rebar corrosion, concrete damage, and ultimately, a rapid decline in the durability of the members and the structure [1–3] . Rebar corrosion can also affect the  \nfatigue performance of RC structures, such as bridges [4] . As an alternative to prevent the deterioration of the durability of RC structures owing to salt damage, the application of fiber-reinforced polymer (FRPs) as concrete reinforcement instead of the corrosion-prone rebar is being researched [5–7] .","cbCail1ygiXHZ9QO","https://ap.wps.com/l/cbCail1ygiXHZ9QO","pdf",7332301,28,"English","# Introduction\n## Seismic deterioration of RC structures in marine environments\n## Motivation for FRP reinforcement instead of corrodible rebar\n## Development trends: bar-type vs grid-type FRP reinforcement","[{\"question\":\"What reinforcement system is evaluated in this study?\",\"answer\":\"The study evaluates concrete walls reinforced with grid-type carbon FRP (CFRP), also comparing their response with reinforced concrete (RC) walls.\"},{\"question\":\"Which experimental variables control the behavior of the carbon-grid reinforced walls?\",\"answer\":\"The variables are the ratio of the carbon-grid anchorage length in the foundation to the wall length, and the axial force ratio.\"},{\"question\":\"How does anchorage length ratio and axial force ratio affect the crushing-load level?\",\"answer\":\"The load at compression-edge cover concrete crushing increases by 1.10 times with increasing axial force ratio and decreases by 0.96 times as the anchorage length ratio decreases.\"}]","Evaluation of the Seismic Behavior of Carbon-Grid-Reinforced Walls with Varying Anchorage and Axial Load Ratios | PDF",1790766258,71,[147,151,155,159],{"page_no":8,"url":148,"width":149,"height":150},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/004d8f34e5069b063ef40a66e65e305f.webp",983,1390,{"page_no":14,"url":152,"width":153,"height":154},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/13b1b63fc53cf97fe716e3f9ef23f474.webp",982,1388,{"page_no":81,"url":156,"width":157,"height":158},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/1fde10a4a8cc978914e2fbb1ddec09db.webp",981,1387,{"page_no":19,"url":160,"width":161,"height":162},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/c37e8802b965ecad59f426c4068383bc.webp",980,1385]