[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-466552-105":59,"doc-detail-466552-en":130},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":123,"head_meta":125,"extra_data":127,"updated_unix":129},105,"en","evaluation-of-pearlite-steel-thermite-weldments-hydrogen-degradation-for-application-of-additively-manufactured-crack-resistant-material-inserts","Evaluation of Pearlite Steel Thermite Weldments’ Hydrogen Degradation for Application of Additively Manufactured Crack-Resistant Material Inserts","","Comprehensive investigations assess the serviceability of pearlite (R260) steel and, specifically, the service behavior of its welded joints during long-term exposure to hydrogen environments for additive manufacturing applications. The study emphasizes estimating durability and analyzing hydrogen influence during service. Hydrogen absorption during welding and subsequent operation significantly increases fatigue and promotes brittle fracture. Hydrogen-saturated specimens form fatigue cracks at fewer cycles, show faster critical fracture, reduced fracture toughness, and orientation-dependent fracture toughness in rail-derived samples.",{"@graph":69,"@context":122},[70,84,105],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/evaluation-of-pearlite-steel-thermite-weldments-hydrogen-degradation-for-application-of-additively-manufactured-crack-resistant-material-inserts/466552/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/evaluation-of-pearlite-steel-thermite-weldments-hydrogen-degradation-for-application-of-additively-manufactured-crack-resistant-material-inserts/466552.png","ImageObject",300,407,{"name":92,"@type":93},"Mabel","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-20","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":34},"InteractionCounter",{"@type":104},"ViewAction",{"@type":106,"mainEntity":107},"FAQPage",[108,114,118],{"name":109,"@type":110,"acceptedAnswer":111},"What material and welded joint does the study evaluate?","Question",{"text":112,"@type":113},"The study evaluates pearlite (R260) steel and the serviceability of its thermite-welded joints during long-term operation in hydrogen-containing environments.","Answer",{"name":115,"@type":110,"acceptedAnswer":116},"How does hydrogen influence fatigue crack initiation and propagation?",{"text":117,"@type":113},"Hydrogen absorbed during welding and service leads to fatigue and brittle fractures, enabling the desired fatigue crack to form at fewer cycles under the same dynamic load. Hydrogen content also affects crack propagation.",{"name":119,"@type":110,"acceptedAnswer":120},"How do hydrogenated and non-hydrogenated specimens compare in fracture behavior?",{"text":121,"@type":113},"Critical fracture occurs faster in hydrogenated specimens than in non-hydrogenated ones, and hydrogenated specimens exhibit lower fracture toughness.","https://schema.org",{"og:url":83,"og:type":124,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":126,"canonical":83},"index,follow",{"doc_id":128,"site_id":62},466552,1791523923,{"code":4,"msg":5,"data":131},{"doc_id":128,"user_id":132,"nickname":92,"user_avatar":133,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":134,"file_id":135,"file_url":136,"file_type":137,"file_size":138,"view_count":34,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":139,"language":140,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":67,"update_tm":144,"read_time":145,"preview_page_count":19,"preview_urls":146},7971474920318,"https://ap-avatar.wpscdn.com/avatar/74000ee537e6b0ca360?x-image-process=image/resize,m_fixed,w_180,h_180&k=1788430171632181674","Article  \nEvaluation of Pearlite Steel Thermite Weldments’ Hydrogen Degradation for Application of Additively Manufactured Crack-Resistant Material Inserts  \nMichał Kawiak 1, Alexander I. Balitskii 1,2, *, Marcin A. Królikowski 1, Valentina O. Balitska 3 and Jakub M. Dowejko 4  \nAcademic Editors: Shengci Li and Zhigang Wang  \nReceived: 25 November 2025  \nRevised: 16 December 2025  \nAccepted: 18 December 2025  \nPublished: 22 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \n1 Department of Mechanical Engineering and Mechatronics, West Pomeranian University of Technology in Szczecin, 19 Piastow Av., 70-310 Szczecin, Poland; [michal.kawiak@zut.edu.pl](michal.kawiak@zut.edu.pl) (M.K.); [marcin.krolikowski@zut.edu.pl](marcin.krolikowski@zut.edu.pl) (M.A.K.)  \n2 Department of Strength of the Materials and Structures in Hydrogen-Containing Environments, Karpenko Physico-Mechanical Institute, National Academy of Sciences of Ukraine, 5 Naukova Str., 79601 Lviv, Ukraine  \n3 Department of Physics and Chemistry of Combustion, Lviv State University of Life Safety, 35 Kleparivska, 79000 Lviv, Ukraine; [vbalitska@yahoo.com](vbalitska@yahoo.com)  \n4 Institute of Management, University of Szczecin, Cukrowa 8, 71-004 Szczecin, Poland  \n* Correspondence: [abalicki@zut.edu.pl](abalicki@zut.edu.pl)  \nAbstract  \nComprehensive investigations of the serviceability of pearlite (R260) steel have been performed and, especially, of the serviceability of their welded joints (WJ) during long-term operation in hydrogen-containing environments for application in additive manufacturing technology. It is important to estimate the durability of these steels and their WJ in hydrogen and develop the procedures of analysis of the influence of hydrogen during long-term operation. It has been experimentally observed that hydrogen absorbed (0.4 . . . 0.8 ppm) by the pearlite (R260) steel while welding, and subsequent operation thereof, exercises considerable influence on fatigue and brittle fractures of the constructions from which they are manufactured. Accordingly, in hydrogen-saturated (up to 4.7 ppm) specimens, the desired fatigue crack can be obtained at a considerably lower number of cycles of the same dynamic load than in non-hydrogenated ones. Increased hydrogen content can also affect crack propagation. Tests have shown that critical fracture occurs faster in hydrogenated specimens (46.6 MPa m0.5 ) than in non-hydrogenated ones. Also, hydrogenated specimens exhibit lower fracture toughness than their non-hydrogenated counterparts. Finally, it has been demonstrated that the fracture toughness of specimens taken from rail negligibly (49.7 . . . 50.7 MPa m0.5 ) depend on their orientation (L–S or S–L) .  \nKeywords: hydrogen; fracture toughness; brittle cracking; thermite welding; tram rails  \n1. Introduction  \nNumerous instances of cracking that occur during welding of rails as well as their further operation indicate that the problem is still common and current. On the other hand, as far as tests required for tram rails (made from perlite steels) are concerned, the EN 13674-1+A1 [1–14] standard does not provide for brittle cracking tests. Lacking proper knowledge, one cannot predict the behaviour of rails operating in each environment and under dynamic loading and ambient temperatures.  \nTherefore, conducting brittle cracking tests for such rails proves relevant, especially whenever the safety of passengers is involved. Despite considerable development in mod-  \nern technology in the thermite welding of rails (based on the thermodynamic principles of the thermite reaction and such characteristics as adiabatic temperatures and heat realisation), especially in terms of rail material, thermite mixtures, equipment, and weld control [3,4], the instances of rail cracking still occur in the course ","cbCainekmsgf6sRR","https://ap.wps.com/l/cbCainekmsgf6sRR","pdf",2796120,18,"English","# Introduction\n## Background and motivation\n## Standards and relevance of tests\n## Observed cracking patterns","[{\"question\":\"What material and welded joint does the study evaluate?\",\"answer\":\"The study evaluates pearlite (R260) steel and the serviceability of its thermite-welded joints during long-term operation in hydrogen-containing environments.\"},{\"question\":\"How does hydrogen influence fatigue crack initiation and propagation?\",\"answer\":\"Hydrogen absorbed during welding and service leads to fatigue and brittle fractures, enabling the desired fatigue crack to form at fewer cycles under the same dynamic load. Hydrogen content also affects crack propagation.\"},{\"question\":\"How do hydrogenated and non-hydrogenated specimens compare in fracture behavior?\",\"answer\":\"Critical fracture occurs faster in hydrogenated specimens than in non-hydrogenated ones, and hydrogenated specimens exhibit lower fracture toughness.\"}]","Evaluation of Pearlite Steel Thermite Weldments’ Hydrogen Degradation for Application of Additively Manufactured Crack-Resistant Material Inserts | PDF",1790771460,45,[147,151,155,159],{"page_no":8,"url":148,"width":149,"height":150},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/105863c1ca9cf3c82ebea85f5d39d5c5.webp",983,1390,{"page_no":14,"url":152,"width":153,"height":154},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/336f07ec555debe77673e723a41fc610.webp",982,1388,{"page_no":81,"url":156,"width":157,"height":158},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/6bdc3adb49e02bcc4c9e9554e480fee9.webp",981,1387,{"page_no":19,"url":160,"width":161,"height":162},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/43de0dab987238f1ddf1eb8ff2103366.webp",980,1385]