[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-458686-105":59,"doc-detail-458686-en":131},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":124,"head_meta":126,"extra_data":128,"updated_unix":130},105,"en","elucidating-the-degradation-behavior-of-a-25-cm2-pure-water-fed-non-precious-metal-anion-exchange-membrane-water-electrolyzer-cell","Elucidating the Degradation Behavior of a 25 cm2 Pure-Water-Fed Non-Precious Metal Anion Exchange Membrane Water Electrolyzer Cell","","Anion exchange membrane water electrolysis (AEMWE) offers a route to hydrogen in a carbon-neutral economy, yet durability limits competitiveness. This study analyzes the degradation behavior of a 25 cm2 AEMWE cell using non-precious metal catalysts and pure-water feed under a short-term durability test. Polarization curves and electrochemical impedance spectroscopy, supported by scanning electron microscopy and energy-dispersive X-ray spectroscopy, reveal performance losses and low stability mainly from anode and anode–membrane interfacial degradation. Ionomer breakdown, reduced hydroxide conductivity, and catalyst-layer mechanical instability are identified as key drivers, informing strategies to improve pure-water-fed AEMWE efficiency and durability.",{"@graph":69,"@context":123},[70,84,106],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/elucidating-the-degradation-behavior-of-a-25-cm2-pure-water-fed-non-precious-metal-anion-exchange-membrane-water-electrolyzer-cell/458686/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/elucidating-the-degradation-behavior-of-a-25-cm2-pure-water-fed-non-precious-metal-anion-exchange-membrane-water-electrolyzer-cell/458686.png","ImageObject",300,407,{"name":92,"@type":93},"Aran","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-02","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":105},"InteractionCounter",{"@type":104},"ViewAction",13,{"@type":107,"mainEntity":108},"FAQPage",[109,115,119],{"name":110,"@type":111,"acceptedAnswer":112},"What degradation mechanisms are identified as key to performance loss in pure-water-fed AEMWE?","Question",{"text":113,"@type":114},"The study identifies ionomer degradation that reduces hydroxide ion conductivity, along with degradation at the anode and at the anode–membrane interface. Catalyst-layer mechanical stability issues also contribute to reduced efficiency and stability.","Answer",{"name":116,"@type":111,"acceptedAnswer":117},"Why is durability important for scaling AEMWE technology?",{"text":118,"@type":114},"Durability is described as a major limiting factor for scale-up and commercialization. Improving cell durability is necessary to make AEMWE competitive for industrial use.",{"name":120,"@type":111,"acceptedAnswer":121},"How does the study experimentally assess degradation behavior?",{"text":122,"@type":114},"It uses polarization curves and electrochemical impedance spectroscopy to track efficiency and stability changes. Scanning electron microscopy and energy-dispersive X-ray spectroscopy are applied to identify degradation-related factors affecting the cell.","https://schema.org",{"og:url":83,"og:type":125,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":127,"canonical":83},"index,follow",{"doc_id":129,"site_id":62},458686,1790885055,{"code":4,"msg":5,"data":132},{"doc_id":129,"user_id":133,"nickname":92,"user_avatar":134,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":135,"file_id":136,"file_url":137,"file_type":138,"file_size":139,"view_count":105,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":140,"language":141,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":142,"faqs":143,"seo_title":144,"seo_description":67,"update_tm":145,"read_time":41,"preview_page_count":19,"preview_urls":146},137455076865,"https://ap-avatar.wpscdn.com/davatar_29158cc5080c5b710cf443261637dec0","RESEARCH ARTICLE  \n[www.small-journal.com](www.small-journal.com)  \nElucidating the Degradation Behavior of a 25 cm2 Pure-Water-Fed Non-Precious Metal Anion Exchange Membrane Water Electrolyzer Cell  \nMichelle S. Lemcke,* Robert Göckeritz, Alexander Müller, Kerstin Witte-Bodnar, Wolfram Münchgesang, and Michael Bron  \nAnion exchange membrane water electrolysis (AEMWE) has become a promising technology for generating hydrogen in a carbon-neutral economy. However, its competitiveness is currently limited by the low durability of AEMWE systems. To increase its durability and to advance its industrial application, this study examines the degradation behavior of a 25 cm2 AEMWE cell utilizing non-precious metal catalysts and pure water feed in a short-term durability test. Polarization curves and electrochemical impedance spectroscopy, along with scanning electron microscopy and energy-dispersive X-ray spectroscopy, are employed to identify factors aﬀecting cell eﬃciencyand stability. The pure-water-fed AEMWE cell exhibits high performance losses and low stability that is mainly related to degradation in the anode and at the interface of anode and membrane. Ionomer degradation, reducing hydroxide ion conductivity, and mechanical stability of the catalyst layer, isidentiﬁed as the key factor decreasing cell eﬃciency and stability during pure water operation. The ﬁndings aim to guide the development of strategies to enhance cell performance and durability of pure-water-fed AEMWE.  \n1. Introduction  \nHydrogen production through water splitting powered by renewable energies is key to realizing a carbon-neutral economy. Among the various electrolyzer technologies, anion exchange membrane water electrolysis (AEMWE) has attracted considerable attention due to its potential for costeﬀective and eﬃcient hydrogen production. Combining the advantages of alkaline electrolysis (AEL) and proton exchange membrane water electrolysis (PEMWE), AEMWE is featured by a compact zero-gap cell design utilizing an anion-selective polymer membrane, non-precious metal catalysts and other inexpensive materials for electrolyzer components due to the alkaline environment. This reduces costs compared to PEMWE while enabling advantages of PEMWE such as high current densities and variable-load operation which is beneﬁcial when powered by wind and solar energy.[1–8]  \nM. S. Lemcke, W. Münchgesang Electrochemical Analytics  \nFraunhofer Institute for Wind Energy Systems IWES  \n27572 Bremerhaven, Germany [E-mail:](E-mail: michelle.sophie.lemcke@iwes.fraunhofer.de)[ michelle.sophie.lemcke@iwes.fraunhofer.de](E-mail: michelle.sophie.lemcke@iwes.fraunhofer.de)  \nM. S. Lemcke, M. Bron Institute of Chemistry  \nMartin Luther University Halle-Wittenberg 06120 Halle (Saale), Germany  \nR. Göckeritz, A. Müller, K. Witte-Bodnar Material Diagnostics for H2 Technologies  \nFraunhofer Institute for Microstructure of Materials and Systems IMWS 06120 Halle (Saale), Germany  \nK. Witte-Bodnar  \nApplied Biosciences and Process Engineering, Hochschule Anhalt University of Applied Science  \n06366 Köthen, Germany  \nThe ORCID identiﬁcation number(s) for the author(s) of this article  \ncan be found under [https://doi.org/10.1002/smll.202506262](https://doi.org/10.1002/smll.202506262)[ ](https://doi.org/10.1002/smll.202506262)© 2025 The Author(s) . Small published by Wiley-VCH GmbH. This is an open access article under the terms of the Creative Commons Attribution License, which permits use, distribution and reproduction in any medium, provided the original work is properly cited.  \nDOI: 10.1002/smll.202506262  \nNevertheless, further research and development is still required to advance the AEMWE technology. A major limiting factor for the scale-up and commercialization of AEMWE is the durability of the system. [6,9,10] Recent proposals ofthe Clean Hydrogen Partnership aim to reduce electricity consumption and capital cost, while increasing the nominal current density and lifetime (see Table 1)","cbCaiiZYYKIg0dq5","https://ap.wps.com/l/cbCaiiZYYKIg0dq5","pdf",7489467,12,"English","# Introduction\n## Hydrogen production and AEMWE context\n## Durability as a limiting factor\n## Pure-water operation challenges\n## Related studies and performance targets","[{\"question\":\"What degradation mechanisms are identified as key to performance loss in pure-water-fed AEMWE?\",\"answer\":\"The study identifies ionomer degradation that reduces hydroxide ion conductivity, along with degradation at the anode and at the anode–membrane interface. Catalyst-layer mechanical stability issues also contribute to reduced efficiency and stability.\"},{\"question\":\"Why is durability important for scaling AEMWE technology?\",\"answer\":\"Durability is described as a major limiting factor for scale-up and commercialization. Improving cell durability is necessary to make AEMWE competitive for industrial use.\"},{\"question\":\"How does the study experimentally assess degradation behavior?\",\"answer\":\"It uses polarization curves and electrochemical impedance spectroscopy to track efficiency and stability changes. Scanning electron microscopy and energy-dispersive X-ray spectroscopy are applied to identify degradation-related factors affecting the cell.\"}]","Elucidating the Degradation Behavior of a 25 cm2 Pure-Water-Fed Non-Precious Metal Anion Exchange Membrane Water Electrolyzer Cell | PDF",1790754084,[147,151,155,159],{"page_no":8,"url":148,"width":149,"height":150},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/ed89ffa3575bbc5184a4ae688b5fb5fb.webp",983,1291,{"page_no":14,"url":152,"width":153,"height":154},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/5f772d1e08b38a0d348c7c05b6753298.webp",982,1290,{"page_no":81,"url":156,"width":157,"height":158},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/a125a3d28053830f095d58e0c1cdbaee.webp",981,1289,{"page_no":19,"url":160,"width":161,"height":162},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/8919239f72ad26946b617a5b17330ca8.webp",980,1287]