[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-465922-105":59,"doc-detail-465922-en":130},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":123,"head_meta":125,"extra_data":127,"updated_unix":129},105,"en","effects-of-solid-solution-heat-treatment-on-the-corrosion-behavior-of-800h-used-in-fourth-generation-nuclear-power-generators","Effects of Solid Solution Heat Treatment on the Corrosion Behavior of 800H Used in Fourth-Generation Nuclear Power Generators","","Incoloy 800H is a key structural alloy for heat-exchange tubes in Generation IV nuclear power systems, where corrosion resistance directly impacts performance optimization and safe operation. The study examines the solid solution heat treatment–microstructure–corrosion resistance link through electrochemical corrosion methods and morphological characterization. Results show 1120 °C is insufficient, causing uneven grain enlargement and undissolved Cr-carbides and leading to fast corrosion. At 1150 °C, grain uniformity improves and Cr-carbides dissolve, giving the best corrosion resistance, while 1180 °C promotes excessive grain growth and severe intergranular corrosion.",{"@graph":69,"@context":122},[70,84,105],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/effects-of-solid-solution-heat-treatment-on-the-corrosion-behavior-of-800h-used-in-fourth-generation-nuclear-power-generators/465922/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/effects-of-solid-solution-heat-treatment-on-the-corrosion-behavior-of-800h-used-in-fourth-generation-nuclear-power-generators/465922.png","ImageObject",300,407,{"name":92,"@type":93},"นรินทร์","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-19","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":52},"InteractionCounter",{"@type":104},"ViewAction",{"@type":106,"mainEntity":107},"FAQPage",[108,114,118],{"name":109,"@type":110,"acceptedAnswer":111},"Why is Incoloy 800H important in Generation IV nuclear power systems?","Question",{"text":112,"@type":113},"It is a structural alloy used for heat-exchange tubes, where stable service depends on its corrosion resistance and thermal strength under demanding conditions.","Answer",{"name":115,"@type":110,"acceptedAnswer":116},"What corrosion outcomes are observed at different solid solution heat treatment temperatures?",{"text":117,"@type":113},"At 1120 °C, corrosion accelerates due to uneven grain enlargement and undissolved Cr-carbides. At 1150 °C, grain growth becomes more uniform and Cr-carbides dissolve, producing the best corrosion resistance. At 1180 °C, excessive grain growth and severe intergranular corrosion occur.",{"name":119,"@type":110,"acceptedAnswer":120},"How does the study connect heat treatment conditions to corrosion resistance?",{"text":121,"@type":113},"It investigates the relationship between heat treatment, resulting microstructure, and corrosion behavior using electrochemical corrosion techniques and morphology characterization.","https://schema.org",{"og:url":83,"og:type":124,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":126,"canonical":83},"index,follow",{"doc_id":128,"site_id":62},465922,1790813217,{"code":4,"msg":5,"data":131},{"doc_id":128,"user_id":132,"nickname":92,"user_avatar":133,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":134,"file_id":135,"file_url":136,"file_type":137,"file_size":138,"view_count":52,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":139,"language":140,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":67,"update_tm":144,"read_time":36,"preview_page_count":19,"preview_urls":145},2336475104957,"https://ap-avatar.wpscdn.com/avatar/22000c4c6bd8a5076e1?x-image-process=image/resize,m_fixed,w_180,h_180&k=1787554080175789136","Article  \nEffects of Solid Solution Heat Treatment on the Corrosion Behavior of 800H Used in Fourth-Generation Nuclear Power Generators  \nYu Liu 1,2,3,*, Xiaoyuan Guo 1, Min Wang 1, Kaixing Yao 1, Huiqing Dong 1, Yafan Li 1, Zhidong Wang 2, Feng Wang 2 and Rui Luo 1, *  \nAcademic Editor: Costica Bejinariu  \nReceived: 2 December 2025  \nRevised: 18 December 2025  \nAccepted: 26 December 2025  \nPublished: 31 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \n1 School of Materials Science & Engineering, Jiangsu University, Zhenjiang 212013, China; [13284620466@163.com](13284620466@163.com) (X.G.); [w16606732729@163.com](w16606732729@163.com) (M.W.); [19741706911@163.com](19741706911@163.com) (K.Y.); [m19859536889@163.com](m19859536889@163.com) (H.D.); [lifeyfan@163.com](lifeyfan@163.com) (Y.L.)  \n2 Jiangsu Yinhuan Precision Steel Pipe Co., Ltd., Yixing 214200, China; [wzdybyq@163.com](wzdybyq@163.com) (Z.W.); [wfyx1988@163.com](wfyx1988@163.com) (F.W.)  \n3 Jiangsu Key Laboratory of Advanced Structural Materials and Application Technology, Nanjing Institute of Technology, Nanjing 211167, China  \n* [Correspondence: yliu5468@ujs.edu.cn](Correspondence: yliu5468@ujs.edu.cn) (Y.L.); [luoruiweiyi@163.com](luoruiweiyi@163.com) (R.L.)  \nAbstract  \nIncoloy 800H is important structural alloy for heat exchange tubes of Generation IV nuclear power systems. Revealing the key heat treatment effects on the microstructure and corrosion behavior of 800H is a key issue for its performance optimization and safe application in IV nuclear power industries. This work investigated the solid solution heat treatment–microstructure–corrosion resistance relationship using various electrochemical corrosion techniques and morphology characterizations. The results showed that 1120 ◦ C was an insufficient solid solution heat treatment temperature for 800H, at which 800H demonstrated uneven enlargement of grains and undissolved Cr-carbides, which resulted in fast corrosion. 800H demonstrated even growth of grains with best grain uniformity and dissolution of Cr-carbides at 1150 ◦ C, thus showing the best corrosion resistance. However, the further increase in solid solution temperature to 1180 ◦ C resulted in excessive grain growth and severe intergranular corrosion (IGC) attack. This work deepened the understanding of the corrosion mechanism of 800H and provided data for its performance optimization.  \nKeywords: 800H; corrosion resistant performance; heat treatment; microstructure  \n1. Introduction  \nNuclear energy, as a clean, safe, efficient, and stable strategic energy source, plays an extremely important role in optimizing energy structure and ensuring energy security. Fourth-generation nuclear energy has the outstanding advantages of high safety and efficiency, low investment, low waste generation, and a stronger nuclear non-proliferation capabilities through technological innovation, etc. It has revolutionary innovations compared with the previous three generations of nuclear power plants and is the only way to solve the contradiction between the continuous growth of energy and the greenhouse effect caused by the consumption of petrochemical fuels today [1–4] . The steam generator is the core equipment for the pressure boundary of the first/second loop of a nuclear power plant. It is not only the hub for efficient conversion of nuclear energy to electrical energy but also an important barrier to ensure the safe operation of the nuclear power  \nplant and prevent the leakage of radioactive fission products. The heat transfer tube is a key component in the steam generator. The historical operating experience of nuclear reactors shows that more than half of the accidents with unit failure rates are caused by heat exchange tubes [5–8] . The increase in the total installed capacity of IV nuclear","cbCaicUzPxkBMsV7","https://ap.wps.com/l/cbCaicUzPxkBMsV7","pdf",4393681,16,"English","# Abstract\n# Keywords\n# 1. Introduction","[{\"question\":\"Why is Incoloy 800H important in Generation IV nuclear power systems?\",\"answer\":\"It is a structural alloy used for heat-exchange tubes, where stable service depends on its corrosion resistance and thermal strength under demanding conditions.\"},{\"question\":\"What corrosion outcomes are observed at different solid solution heat treatment temperatures?\",\"answer\":\"At 1120 °C, corrosion accelerates due to uneven grain enlargement and undissolved Cr-carbides. At 1150 °C, grain growth becomes more uniform and Cr-carbides dissolve, producing the best corrosion resistance. At 1180 °C, excessive grain growth and severe intergranular corrosion occur.\"},{\"question\":\"How does the study connect heat treatment conditions to corrosion resistance?\",\"answer\":\"It investigates the relationship between heat treatment, resulting microstructure, and corrosion behavior using electrochemical corrosion techniques and morphology characterization.\"}]","Effects of Solid Solution Heat Treatment on the Corrosion Behavior of 800H Used in Fourth-Generation Nuclear Power Generators | PDF",1790770263,[146,150,154,158],{"page_no":8,"url":147,"width":148,"height":149},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/13688d1efa135ac2f04dc39ea41dd895.webp",983,1390,{"page_no":14,"url":151,"width":152,"height":153},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/3cc1d92430845c79cd5c91b3f98ab06c.webp",982,1388,{"page_no":81,"url":155,"width":156,"height":157},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/2df02d2cfdcf8c23e2da6f5472243bcb.webp",981,1387,{"page_no":19,"url":159,"width":160,"height":161},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/bd5ce48a549e2e5974a4335681da7821.webp",980,1385]