[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-466526-105":59,"doc-detail-466526-en":130},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":123,"head_meta":125,"extra_data":127,"updated_unix":129},105,"en","effect-of-solution-temperature-on-corrosion-behavior-of-ti-6al-4zr-3nb-11mo-1sn-1v-alloy-in-hydrochloric-acid-solution","Effect of Solution Temperature on Corrosion Behavior of Ti-6Al-4Zr-3Nb-1.1Mo-1Sn-1V Alloy in Hydrochloric Acid Solution","","Ti-6Al-4Zr-3Nb-1.1Mo-1Sn-1V (Ti90) alloy is widely applied in marine engineering and oil and gas extraction for its strength, impact toughness, and corrosion resistance. Corrosion behavior after solution treatment at 750 °C, 900 °C, 940 °C, and 960 °C in 5 M hydrochloric acid was assessed using OCP, potentiodynamic polarization, electrochemical impedance spectroscopy, static immersion, and surface characterization. Electrochemical results show increasing corrosion resistance with higher solid-solution temperature, matching immersion trends. Corrosion morphology indicates stronger α-phase decomposition than β-phase, governed by β-phase volume fraction and α-phase size.",{"@graph":69,"@context":122},[70,84,105],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/effect-of-solution-temperature-on-corrosion-behavior-of-ti-6al-4zr-3nb-11mo-1sn-1v-alloy-in-hydrochloric-acid-solution/466526/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/effect-of-solution-temperature-on-corrosion-behavior-of-ti-6al-4zr-3nb-11mo-1sn-1v-alloy-in-hydrochloric-acid-solution/466526.png","ImageObject",300,407,{"name":92,"@type":93},"Dipper","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-10-31","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":34},"InteractionCounter",{"@type":104},"ViewAction",{"@type":106,"mainEntity":107},"FAQPage",[108,114,118],{"name":109,"@type":110,"acceptedAnswer":111},"What alloy and environment are investigated in this study?","Question",{"text":112,"@type":113},"The study focuses on Ti-6Al-4Zr-3Nb-1.1Mo-1Sn-1V (Ti90) alloy exposed to 5 M hydrochloric acid after solution treatment at different temperatures.","Answer",{"name":115,"@type":110,"acceptedAnswer":116},"Which methods are used to evaluate the corrosion behavior?",{"text":117,"@type":113},"Corrosion behavior is examined using OCP, potentiodynamic polarization, EIS, static immersion tests, and surface characterization.",{"name":119,"@type":110,"acceptedAnswer":120},"How does solid-solution temperature affect corrosion resistance?",{"text":121,"@type":113},"Electrochemical and immersion results indicate that corrosion resistance increases as solid-solution temperature rises.","https://schema.org",{"og:url":83,"og:type":124,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":126,"canonical":83},"index,follow",{"doc_id":128,"site_id":62},466526,1791021985,{"code":4,"msg":5,"data":131},{"doc_id":128,"user_id":132,"nickname":92,"user_avatar":133,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":134,"file_id":135,"file_url":136,"file_type":137,"file_size":138,"view_count":34,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":139,"language":140,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":67,"update_tm":144,"read_time":145,"preview_page_count":19,"preview_urls":146},1374404997633,"https://ap-avatar.wpscdn.com/davatar_a8503ba1806abce46bf441b54a3ca4cd","Article  \nEffect of Solution Temperature on Corrosion Behavior of Ti-6Al-4Zr-3Nb-1.1Mo-1Sn-1V Alloy in Hydrochloric Acid Solution  \nChengliang Mao *, Siyuan Zhang , Silan Li, Jialu Wang, Qian Li * and Weiju Jia *  \nAcademic Editor: Daniel John Blackwood  \nReceived: 31 October 2025  \nRevised: 4 December 2025  \nAccepted: 18 December 2025  \nPublished: 22 December 2025  \nCopyright: © 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.  \nNorthwest Institute for Nonferrous Metal Research, Xi’an 710016, China  \n* [Correspondence: mclustb@163.com](Correspondence: mclustb@163.com) (C.M.); [leeqian0426@hotmail.com](leeqian0426@hotmail.com) (Q.L.); [diana_1025@126.com](diana_1025@126.com) (W.J.)  \nAbstract  \nTi-6Al-4Zr-3Nb-1.1Mo-1Sn-1V (Ti90) alloy is widely used in marine engineering and oil and gas extraction due to its excellent strength, impact toughness, and corrosion resistance. The corrosion behavior of Ti90 alloy after solution treatment at 750 ◦ C, 900 ◦ C, 940 ◦ C, and 960 ◦ C in 5 M hydrochloric acid (HCl) solution was investigated using open-circuit potential (OCP), potentiodynamic polarization, electrochemical impedance spectroscopy (EIS), static immersion tests, and surface characterization. The results of electrochemical tests indicate that the corrosion resistance of Ti90 alloy increases with rising solid solution temperature. The static immersion tests show that the variation trend of the annual corrosion rate at different solid solution temperatures in 5 M HCl solution is consistent with the electrochemical test results. The corrosion morphology of Ti90 alloy reveals that the α phase is more prone to decomposition than the β phase. The corrosion behavior of Ti90 alloy in 5 M HCl solution is mainly influenced by the volume fraction of the β phase and the size of the α phase.  \nKeywords: titanium alloy; microstructure; electrochemical techniques; corrosion behavior  \n1. Introduction  \nTitanium alloy has high corrosion resistance and is often used in harsh service environments. The surface of titanium alloy contains a dense passivation film mainly composed of TiO2, which contributes not only to corrosion resistance but also to biocompatibility [1–5] . This oxide film exhibits strong corrosion resistance in most service environments. In some cases, even if damaged, it can repair itself rapidly. However, the passivation film on titanium alloy faces a relatively high risk of damage in reducing acid solutions. According to the existing literature, the main factors influencing the corrosion behavior of titanium alloys include alloy composition, microstructure characteristics, and usage environment [6–10] .  \nMicrostructure plays a significant role in the corrosion behavior of titanium alloy [2,11] . Titanium alloys subjected to different thermomechanical processing and heat treatment processes exhibit substantial microstructural differences, mainly involving morphological features, grain size, phase content, and even dislocation density [12,13] . The influence of different microstructures on the corrosion resistance of titanium alloys is intricate and complex, leading to inconsistent conclusions among researchers. Wei et al. [14] . investigated the corrosion and passivation behavior of Ti-3Mo alloy in 20 wt.% HCl solution at solution temperatures ranging from 750 ◦ C to 1050 ◦ C. The corrosion rate increased with rising treatment temperature, which was attributed to accelerated corrosion of the passivation  \nfilm above 850 ◦ C and the establishment of micro-galvanic cells at the α/β phase interface. Meng et al. [15] . studied the corrosion resistance of Ti80 alloy annealed from 800 ◦ C to 1040 ◦ C in 5 wt.% HCl solution. As the treatment temperature increased from 800 ◦ C to 960 ◦ C, the corrosion resistance improved. When the annealing temperature reached 1040 ◦ C, the corrosion rate decrea","cbCaim8dl3yvEmOi","https://ap.wps.com/l/cbCaim8dl3yvEmOi","pdf",9377325,15,"English","# Abstract\n# 1. Introduction","[{\"question\":\"What alloy and environment are investigated in this study?\",\"answer\":\"The study focuses on Ti-6Al-4Zr-3Nb-1.1Mo-1Sn-1V (Ti90) alloy exposed to 5 M hydrochloric acid after solution treatment at different temperatures.\"},{\"question\":\"Which methods are used to evaluate the corrosion behavior?\",\"answer\":\"Corrosion behavior is examined using OCP, potentiodynamic polarization, EIS, static immersion tests, and surface characterization.\"},{\"question\":\"How does solid-solution temperature affect corrosion resistance?\",\"answer\":\"Electrochemical and immersion results indicate that corrosion resistance increases as solid-solution temperature rises.\"}]","Effect of Solution Temperature on Corrosion Behavior of Ti-6Al-4Zr-3Nb-1.1Mo-1Sn-1V Alloy in Hydrochloric Acid Solution | PDF",1790771414,38,[147,151,155,159],{"page_no":8,"url":148,"width":149,"height":150},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/f8828be1ac60f5a452d3d72e12ab0a69.webp",983,1390,{"page_no":14,"url":152,"width":153,"height":154},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/9c2f495b166e4b87321edf27f84f4147.webp",982,1388,{"page_no":81,"url":156,"width":157,"height":158},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/bca6e7c6e10182807fcd5244f580fb3e.webp",981,1387,{"page_no":19,"url":160,"width":161,"height":162},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/8b17dfc5adbb476c11b1f07cba51e530.webp",980,1385]