[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-497512-105":59,"doc-detail-497512-en":131},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":124,"head_meta":126,"extra_data":128,"updated_unix":130},105,"en","effect-of-cmas-composition-on-hot-corrosion-behavior-of-gadolinium-zirconate-thermal-barrier-coating-materials","Effect of CMAS Composition on Hot Corrosion Behavior of Gadolinium Zirconate Thermal Barrier Coating Materials","","Resistance of synthesized pyrochlore-type Gd2Zr2O7 bulk specimens to four CMAS (calcium-magnesium-aluminosilicate) compositions at different temperatures was evaluated. Reaction products were characterized by X-ray diffraction, while penetration depths were measured using scanning electron microscopy. Results show a dense reaction layer mainly containing Ca2Gd8(SiO4)6O2 and a cubic fluorite phase, with unreacted CMAS in a transition layer. Infiltration depth changed only slightly with temperature, whereas reaction-layer thickness and transition-layer morphology varied markedly. The CaO-lean CMAS caused the most severe degradation; CaSO4 and CaCO3 effects were minimal, and Gd in the cubic fluorite phase depended on temperature and Ca:Si molar ratio.",{"@graph":69,"@context":123},[70,84,106],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/effect-of-cmas-composition-on-hot-corrosion-behavior-of-gadolinium-zirconate-thermal-barrier-coating-materials/497512/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/effect-of-cmas-composition-on-hot-corrosion-behavior-of-gadolinium-zirconate-thermal-barrier-coating-materials/497512.png","ImageObject",300,407,{"name":92,"@type":93},"gewufjwa","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-12","2026-10-02",true,{"@type":102,"interactionType":103,"userInteractionCount":105},"InteractionCounter",{"@type":104},"ViewAction",21,{"@type":107,"mainEntity":108},"FAQPage",[109,115,119],{"name":110,"@type":111,"acceptedAnswer":112},"What was the main objective of the study on Gd2Zr2O7?","Question",{"text":113,"@type":114},"To investigate how different CMAS compositions affect the hot corrosion behavior of pyrochlore-type Gd2Zr2O7 bulk specimens at different temperatures.","Answer",{"name":116,"@type":111,"acceptedAnswer":117},"How were the reaction products and penetration depths analyzed?",{"text":118,"@type":114},"Reaction products were identified using X-ray diffraction, and penetration depths were examined using scanning electron microscopy.",{"name":120,"@type":111,"acceptedAnswer":121},"Which CMAS composition caused the most severe degradation?",{"text":122,"@type":114},"The sintered sample underwent the most severe degradation by CaO-lean CMAS, while the effects of CaSO4 and CaCO3 were not significant.","https://schema.org",{"og:url":83,"og:type":125,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":127,"canonical":83},"index,follow",{"doc_id":129,"site_id":62},497512,1791093585,{"code":4,"msg":5,"data":132},{"doc_id":129,"user_id":133,"nickname":92,"user_avatar":134,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":135,"file_id":136,"file_url":137,"file_type":138,"file_size":139,"view_count":105,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":140,"language":141,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":142,"faqs":143,"seo_title":144,"seo_description":67,"update_tm":145,"read_time":146,"preview_page_count":19,"preview_urls":147},3985747882900,"https://ap-avatar.wpscdn.com/davatar_9964176cb1d06d4a9deccf72a44ae3dc","Effect of CMAS Composition on Hot Corrosion Behavior of Gadolinium Zirconate Thermal Barrier Coating Materials  \nWenzhuo Deng, Jeffrey W. Fergus  \nMaterials Research and Education Center, Auburn University, Auburn, Alabama 36849, USA  \nAbstract: The resistance of synthesized pyrochlore-type Gd2Zr2O7 bulk specimens to four calciummagnesium aluminosilicate (CMAS) compositions at different temperatures was investigated. Thereaction products were identified by x-ray diffraction and penetration depths were examined using scanning electron microscopy. A dense reaction layer is comprised mainly of Ca2Gd8(SiO4)6O2 and a cubic fluorite phase formed during the CMAS attack, and some unreacted CMAS was found in a transition layer below the reaction layer. The overall infiltration depth changed slightly with temperature, however, the thickness of the reaction layer and the morphology of the transition layer varied distinctly with temperature. The sintered sample underwent the most severe degradation by the CaO-lean CMAS, whereas the effect of CaSO4 and CaCO3 was not significant. Moreover, the Gd content of the ZrO2-based cubic fluorite phase depends on the temperature and the molar ratio of Ca:Si in the CMAS.  \nIntroduction  \nThe efficiency of gas turbine engines increases with increasing operating temperature. Thermal barrier coatings (TBCs) act as thermal insulators for metallic fans and vanes, which allows for a higher operating temperature and thus increases the thrust-to-weight ratio of the turbine.1 Yttria-stabilized zirconia (YSZ) with the intermediate t’-tetragonal phase has been widely used in aero engines for decades owing to its excellent mechanical and chemical properties during thermal cycling.2 However, YSZ cannot meet the requirements of modern turbines, because issues like delamination and spallation due to the phase transformation accompanied with volume changes and poor chemical resistance to molten salts at elevated temperature are detrimental to the performance and shorten the lifetimes of jet engines.3-7 Conversely, the rare earth zirconates, especially gadolinium zirconate (Gd2Zr2O7) with the pyrochlorestructure, which exhibit relatively low thermal expansion coefficient, high-temperature phase stability, and low thermal conductivity, are of great potential.8, 9  \nIn general, TBC materials can be deposited using atmospheric plasma spraying (APS) on the stationary components or electron beam physical vapor deposition (EB-PVD) on the rotating parts of the turbine. The corresponding specific lamellar or columnar structure of APS or EB-PVD deposited coatings with porosities of 10-25% benefits mitigation of stresses and decreases thermal conductivity.10, 11 However, the intersplat pores or intercolumn gaps are the main paths for the infiltration of molten salts during service. The molten salts, which come from sand, dust, volcanic ash and even impurities in the fuel, are mainly composed of calcium-magnesium-alumino-silicate (CMAS) .4 Since Gd2Zr2O7 is a promising alternative TBC material, the influence of CMAS on its performance has been of interest.12-16 Molten CMAS wets the surface, penetrates the pores, and reacts with the pyrochlore material resulting in the establishment of a compact layer composed of a lanthanide-apatite phase, usually in a rod-like shape, and a cubic fluorite phase in a globular form, which is conducive to the suppression of further CMAS permeation.17 The extent of degradation strongly depends on temperature and the composition of CMAS glass. One reason for this dependence is the viscosity of CMAS glass, which has been predicted using software based on models and melt databases,18-21 depends on temperature and affects CMAS  \ncorrosion.4, 19 Furthermore, the compositions and amounts of the cubic fluorite and apatite phases are also significantly affected by the temperature.22  \nAnhydrite (CaSO4) has been reported to penetrate through the entire EB-PVB deposited YSZ top coating from the debris of the ","cbCaifyuys1z4Hzr","https://ap.wps.com/l/cbCaifyuys1z4Hzr","pdf",1327440,13,"English","# Introduction\n# Experimental Procedure\n## Preparation of pyrochlore-type material\n## Hot corrosion tests","[{\"question\":\"What was the main objective of the study on Gd2Zr2O7?\",\"answer\":\"To investigate how different CMAS compositions affect the hot corrosion behavior of pyrochlore-type Gd2Zr2O7 bulk specimens at different temperatures.\"},{\"question\":\"How were the reaction products and penetration depths analyzed?\",\"answer\":\"Reaction products were identified using X-ray diffraction, and penetration depths were examined using scanning electron microscopy.\"},{\"question\":\"Which CMAS composition caused the most severe degradation?\",\"answer\":\"The sintered sample underwent the most severe degradation by CaO-lean CMAS, while the effects of CaSO4 and CaCO3 were not significant.\"}]","Effect of CMAS Composition on Hot Corrosion Behavior of Gadolinium Zirconate Thermal Barrier Coating Materials | PDF",1790958673,33,[148,152,156,160],{"page_no":8,"url":149,"width":150,"height":151},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/d27f58711657ef27079f13ae094013ad.webp",983,1272,{"page_no":14,"url":153,"width":154,"height":155},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/a61409c33508ce1af0ec871e2e7214b3.webp",982,1270,{"page_no":81,"url":157,"width":158,"height":159},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/c69185602465d465e4dd89b696e537ce.webp",981,1269,{"page_no":19,"url":161,"width":162,"height":163},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/d0e25ac207707b2e996bb1b3f33467ba.webp",980,1268]