[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-509296-105":59,"doc-detail-509296-en":130},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":123,"head_meta":125,"extra_data":127,"updated_unix":129},105,"en","development-of-process-for-reduction-in-fines-generation-at-direct-reduced-iron-plant-by-coating-of-magnetite-iron-ore-fines-on-hematite-iron-ore-pellets","Development of process for reduction in fines generation at direct reduced iron plant by coating of magnetite iron ore fines on hematite iron ore pellets","","Iron ore pellet fines generation at direct reduced iron (DRI) plants ranges from 10% to 12% during handling from pelletizing to DRI. Fines formation during handling depends mainly on pellet quality and its abrasion index (AI). Laboratory studies evaluate reducing pellet fines by coating hematite iron ore pellet surfaces with magnetite fines from reduction roasting and by mixing magnetite fines with limestone fines. Coated green pellets were fired in a hearth furnace, and optimum 1.5% magnetite fines reduced fines from 6.8% to 3.2%. Mixed 0.2% limestone and 1.5% magnetite reduced fines to 4.2%, attributed to secondary hematite and Ca-ferrite formation that improves microhardness and overall pellet properties.",{"@graph":69,"@context":122},[70,84,105],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/development-of-process-for-reduction-in-fines-generation-at-direct-reduced-iron-plant-by-coating-of-magnetite-iron-ore-fines-on-hematite-iron-ore-pellets/509296/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/development-of-process-for-reduction-in-fines-generation-at-direct-reduced-iron-plant-by-coating-of-magnetite-iron-ore-fines-on-hematite-iron-ore-pellets/509296.png","ImageObject",300,407,{"name":92,"@type":93},"Emma Wilson","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-06","2026-10-05",true,{"@type":102,"interactionType":103,"userInteractionCount":34},"InteractionCounter",{"@type":104},"ViewAction",{"@type":106,"mainEntity":107},"FAQPage",[108,114,118],{"name":109,"@type":110,"acceptedAnswer":111},"What drives pellet fines generation at the DRI plant?","Question",{"text":112,"@type":113},"Pellet fines generation is mainly driven by abrasion during handling and transporting, and it depends on pellet quality such as the abrasion index (AI), along with raw material type and furnace/handling conditions.","Answer",{"name":115,"@type":110,"acceptedAnswer":116},"How was the coating strategy designed to reduce fines?",{"text":117,"@type":113},"Hematite pellets were coated with magnetite fines, and magnetite fines were also mixed with limestone fines. The coated green pellets were fired in a hearth furnace, varying magnetite (0–2.5%) and limestone fines (0–0.6%).",{"name":119,"@type":110,"acceptedAnswer":120},"What were the best results and why?",{"text":121,"@type":113},"Optimum 1.5% magnetite fines reduced fines generation from 6.8% to 3.2% due to formation of secondary hematite phases at the pellet shell. Mixing 0.2% limestone with 1.5% magnetite reduced fines to 4.2%, linked to secondary hematite and Ca-ferrite formation at the pellet surface.","https://schema.org",{"og:url":83,"og:type":124,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":126,"canonical":83},"index,follow",{"doc_id":128,"site_id":62},509296,1791307931,{"code":4,"msg":5,"data":131},{"doc_id":128,"user_id":132,"nickname":92,"user_avatar":133,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":134,"file_id":135,"file_url":136,"file_type":137,"file_size":138,"view_count":34,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":52,"language":139,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":140,"faqs":141,"seo_title":142,"seo_description":67,"update_tm":143,"read_time":144,"preview_page_count":19,"preview_urls":145},3848291630094,"https://eur-avatar.wpscdn.com/davatar_085a072bc5b1113ac321206ff7593b45","Metall. Res. Technol. 119, 604 (2022)© EDP Sciences, 2022  \n[https://doi.org/10.1051/metal/2022088](https://doi.org/10.1051/metal/2022088)  \n&etchanlurgiclogyal Research  \nAvailable online at:  \n[www.metallurgical-research.org](www.metallurgical-research.org)  \n\n| REGULAR ARTICLE | |\n| --- | --- |\n\nDevelopment of process for reduction in ﬁ nes generation at direct reduced iron plant by coating of magnetite iron ore ﬁneson hematite iron ore pellets  \n*  \nTekkalakote Umadevi , Komala Sivanna Sridhara, Munukuntla Raju, P. Karthik, Rameshwar Sah,  \nMaribasappanavar Basavaraja, and Sanghamesh Desai JSW Steel Limited, Bellary, India  \nReceived: 25 April 2022 / Accepted: 22 September 2022  \nAbstract. Iron ore pellet ﬁnes generation at direct reduced iron (DRI) plant is ranging from 10 to 12% during handlingofthe pellets frompellet planttoDRI plant. Thegeneration ofﬁnes during handling depends onthe quality of the produced pellets, mainly dueto the abrasion index (AI) of the pellet. To reduce the generation of pellet ﬁnes, detailed laboratory studies have been carried out by coatingthe hematite iron ore pellet surfacewith magnetiteﬁnes generated from reduction roasting plant, and mixed magnetite ﬁnes with limestone ﬁnes. The coated green pellets wereﬁred in arising hearth furnace. The magnetiteﬁnes were varied from0to2.5%as coating agent, and limestone ﬁnes was varied from 0 to 0 .6% as coating agent mixed with magnetite ﬁnes. At optimum 1 .5% magnetite ﬁnes as coating agent achieved better pellet properties and reducedtheﬁnes generation from6.8to3.2%due to formation of secondary hematite phases at the pellet shell. With mixed 0 .2% limestone and 1 .5% magnetite ﬁnes reduced pellet ﬁnes generation from6.8to4.2%. Reduction inﬁnes generation with mixedﬁnes was due to formation ofsecondary hematite and Ca-ferrite at the pellet surface. Secondary hematite and Ca ferrite phases having higher microhardness compared to other phases of iron ore pellet. The sequence of micro-hardness of the pellet phases is secondary hematite > Ca-ferrite > primary hematite > magnetite. The secondary hematite and Ca-ferrite formed atthe pellet surface due to coating ofmagnetite as well as magnetite with limestoneﬁnes improved the overall pellet quality and reduced the generation of ﬁnes at DRI plant. Coating of magnetite ﬁnes alone showed better pellet properties with lesser ﬁnes generation compared to coating of mixed limestone and magnetite ﬁnes.  \nKeywords: hematite iron ore pellets / magnetite and limestone ﬁnes / coating / ﬁnes generation / mineralogy / pellet properties  \n1 Introduction  \nThe generation of iron ore pellets ﬁnes during handling/ transporting from induration furnace to user end i.e. DRIplant, Corex and blast furnace, is due to the abrasion. The abrasion resistance of the pellet is indicated by abrasion index (AI) . Iron ore pellet ﬁnes generation at DRI plant is ranging from 10 to 12% . The generation of ﬁnes leads to pellet production loss and reduces the availability of pellet at end user. Generation of the pellet ﬁnes mainly depends on the type & chemistry of raw materials, straight grate induration furnace conditions and type and extent of handling. The temperature proﬁle and type of raw material (hematite and magnetite iron ore), size of the pellets, position of the pellet in the induration furnace and bed level decides the physical and metallurgical properties of the  \n* e-mail: [uma.devi@jsw.in](uma.devi@jsw.in)  \npellets. The bottom layer pellets are weaker pellets and lower tumbler index due to ﬁring of the pellets is downdraft and abrasion indexofthese pellets are higher compared to middle and top layer of the pellets. The larger pellets in the bottom layer were improperly ﬁred, and larger pellets required more residence time [1] . Quality of the pellet as well as surface properties of the pellets mainly decides the pellet ﬁnes generation. It was observed that the magnetite pellets are higher physical and metallurgical properties","cbCaitCPJliMCdWl","https://ap.wps.com/l/cbCaitCPJliMCdWl","pdf",2078522,"English","# Abstract\n# Keywords\n## 1 Introduction\n## Table 1 Chemical analysis\n## Table 2 Size analysis","[{\"question\":\"What drives pellet fines generation at the DRI plant?\",\"answer\":\"Pellet fines generation is mainly driven by abrasion during handling and transporting, and it depends on pellet quality such as the abrasion index (AI), along with raw material type and furnace/handling conditions.\"},{\"question\":\"How was the coating strategy designed to reduce fines?\",\"answer\":\"Hematite pellets were coated with magnetite fines, and magnetite fines were also mixed with limestone fines. The coated green pellets were fired in a hearth furnace, varying magnetite (0–2.5%) and limestone fines (0–0.6%).\"},{\"question\":\"What were the best results and why?\",\"answer\":\"Optimum 1.5% magnetite fines reduced fines generation from 6.8% to 3.2% due to formation of secondary hematite phases at the pellet shell. Mixing 0.2% limestone with 1.5% magnetite reduced fines to 4.2%, linked to secondary hematite and Ca-ferrite formation at the pellet surface.\"}]","Development of process for reduction in fines generation at direct reduced iron plant by coating of magnetite iron ore fines on hematite iron ore pellets | PDF",1791234991,25,[146,150,154,158],{"page_no":8,"url":147,"width":148,"height":149},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/4fbbfac626b96720e40257fa4f72416b.webp",983,1310,{"page_no":14,"url":151,"width":152,"height":153},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/5a5ddb39a2c652c5292cbd4cd7617dbc.webp",982,1309,{"page_no":81,"url":155,"width":156,"height":157},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/065d7718d02cb0062c85c407a6310868.webp",981,1308,{"page_no":19,"url":159,"width":160,"height":161},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/de7b5ce67a26d89abcaade122b0690e8.webp",980,1306]