[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-497708-105":59,"doc-detail-497708-en":131},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":124,"head_meta":126,"extra_data":128,"updated_unix":130},105,"en","design-of-ti2alcysz-tbcs-for-more-efficient-in-resisting-cmas-attack","Design of Ti2AlC/YSZ TBCs for more efficient in resisting CMAS attack","","Ti2AlC is evaluated as a protective-layer material for thermal barrier coatings (TBCs) against calcium–magnesium–alumina–silicate (CMAS) attack. Reliability of Ti2AlC coatings against CMAS corrosion is investigated, and Ti2AlC/YSZ TBCs with improved CMAS resistance are designed. Sprayed Ti2AlC contains impurity phases (TiC, Al2Ti3), whose amount is reduced by optimizing spray distance; corrosion tests show higher resistance than YSZ but long-term exposure causes microstructural degradation and surface formation of Al2O3–TiO2 mixed layers. Pre-oxidation in air or controlled oxygen partial pressure promotes a continuous Al2O3 layer (~630 Pa), and vacuum heat treatment at 867 ℃ for 10 h further supports a compact Al2O3 structure, yielding lower impurity content and higher microstructural stability under CMAS exposure.",{"@graph":69,"@context":123},[70,84,106],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/design-of-ti2alcysz-tbcs-for-more-efficient-in-resisting-cmas-attack/497708/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/design-of-ti2alcysz-tbcs-for-more-efficient-in-resisting-cmas-attack/497708.png","ImageObject",300,407,{"name":92,"@type":93},"Connor ","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-26","2026-10-02",true,{"@type":102,"interactionType":103,"userInteractionCount":105},"InteractionCounter",{"@type":104},"ViewAction",18,{"@type":107,"mainEntity":108},"FAQPage",[109,115,119],{"name":110,"@type":111,"acceptedAnswer":112},"Why is CMAS attack critical for thermal barrier coatings?","Question",{"text":113,"@type":114},"CMAS deposits on blade surfaces, melts at high temperature, penetrates the coating, blocks micropores, and triggers phase transformations and ZrO2 degradation, leading to TBC failure.","Answer",{"name":116,"@type":111,"acceptedAnswer":117},"What role do impurity phases in Ti2AlC coatings play?",{"text":118,"@type":114},"Ti2AlC coatings contain impurity phases such as TiC and Al2Ti3. With long-term CMAS exposure, these impurities contribute to microstructure degradation and promote the formation of an Al2O3–TiO2 mixed layer rather than a compact Al2O3 layer.",{"name":120,"@type":111,"acceptedAnswer":121},"How does pre-oxidation improve CMAS resistance in Ti2AlC/YSZ TBCs?",{"text":122,"@type":114},"Pre-oxidation in air or under controlled oxygen partial pressure increases the formation of a continuous Al2O3 layer on the Ti2AlC surface; an oxygen partial pressure around ~630 Pa is reported to be effective, and a vacuum heat treatment at 867 ℃ for 10 h before pre-oxidation further helps form a compact Al2O3 layer.","https://schema.org",{"og:url":83,"og:type":125,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":127,"canonical":83},"index,follow",{"doc_id":129,"site_id":62},497708,1791033849,{"code":4,"msg":5,"data":132},{"doc_id":129,"user_id":133,"nickname":92,"user_avatar":134,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":135,"file_id":136,"file_url":137,"file_type":138,"file_size":139,"view_count":105,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":56,"language":140,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":141,"faqs":142,"seo_title":143,"seo_description":67,"update_tm":144,"read_time":145,"preview_page_count":19,"preview_urls":146},687207022233,"https://ap-avatar.wpscdn.com/davatar_155a257f0dc6eb9ab79c44ca47cae57d","Journal of Advanced Ceramics  \n 2023, 12(9): 1712–1730 ISSN 2226-4108  \n [https://doi.org/10.26599/JAC.2023.9220781](https://doi.org/10.26599/JAC.2023.9220781) CN 10-1154/TQ  \nResearch Article  \nDesign of Ti2AlC/YSZ TBCs for more efficient in resisting CMAS attack  \nLei Guoa,b,* , Yanyan Lia, Guang Lia,c  \naSchool of Materials Science and Engineering, Tianjin University, Tianjin 300072, China b Tianjin Key Laboratory of Advanced Joining Technology, Key Lab of Advanced Ceramics and Machining Technology, Ministry of Education, Tianjin 300072, China cShanghai Institute of Space Power-Sources, Shanghai 200240, China  \nReceived: May 4, 2023; Revised: June 22, 2023; Accepted: June 24, 2023  \n© The Author(s) 2023.  \nAbstract: Ti2AlC has been demonstrated as the promising protective layer material for thermal barrier coatings (TBCs) against calcium–magnesium–alumina–silicate (CMAS) attack. In this study, the reliability of Ti2AlC coatings against the CMAS corrosion was explored, and new Ti2AlC/YSZ TBCs more efficiently resistant to CMAS were designed. The fabricated Ti2AlC coatings inevitably contain some impurity phases (TiC and Al2Ti3), the contents of which were minimized by optimizing the spraying distance. Corrosion tests revealed that Ti2AlC/YSZ TBCs yielded higher resistance to the CMAS attack than YSZ TBCs, but with long-term exposure to CMAS, the Ti2AlC protective coating exhibited microstructure degradation due to the presence of the impurity phases, which caused the formation of a layer mixed with Al2O3 and TiO2 rather than a continuous compact Al2O3 layer on the surface. Pre-oxidation schemes were designed in air or with a controlled oxygen partial pressure, which revealed that the pre-oxidation at an oxygen partial pressure of ~630 Pa could promote a continuous Al2O3 layer formed on the Ti2AlC protective coating surface. Furthermore, a vacuum heat treatment at 867 ℃ for 10 h before pre-oxidation was beneficial for the formation of the compact Al2O3 layer. Through the above scheme design, new Ti2AlC/YSZ TBCs were obtained, which had reduced impurity phase contents and a pre-oxide layer with an ideal structure on the surface. New TBCs exhibit higher microstructure stability exposed to CMAS and more efficient CMAS resistance.  \nKeywords: thermal barrier coatings (TBCs); calcium–magnesium–alumina–silicate (CMAS); Ti2AlC/ YSZ; pre-oxidation design; corrosion resistance mechanisms  \n1 Introduction  \nAs an important factor to reflect scientific and technological advantages of a country, aero engines have developed rapidly and their thrust-to-weight  \n* Corresponding author.  \nE-mail: [glei028@tju.edu.cn](glei028@tju.edu.cn)  \nratio is increasingly rising, resulting in the working temperature of turbine blades exceeding that of currently used superalloys [1–3] . Thermal barrier coatings (TBCs) technology is a key mechanism for reducing the temperature of alloy blades, which composites thermal insulation ceramic materials to the surface of superalloy blades, and the traditional TBC material is yttria partially stabilized zirconia (YSZ) [4] .  \nHowever, when aircraft flies across volcanoes, deserts, and other areas, environmental particles such as sand and dust, whose main component is calcium– magnesium–alumina–silicate (CMAS), would be ingested into the engine and deposited on blade surfaces [5] . At high temperatures, CMAS melts, penetrates, and blocks coating micropores, reducing strain tolerance. More severely, CMAS infiltration results in tetragonal– monoclinic phase transformation of the coating and precipitation of Y-depleted ZrO2, leading to degradation of the TBCs [6–8] . Therefore, the protection against CMAS corrosion has become an urgent research problem.  \nTo alleviate the CMAS corrosion to TBCs, scholars proposed many protection methods, mainly includingthe following aspects: firstly, modifying the composition of YSZ to promote CMAS crystallization. It has been reported that Cr2O3 and TiO2 can be used as nucleating a","cbCaisfRMQQHdC0H","https://ap.wps.com/l/cbCaisfRMQQHdC0H","pdf",2144138,"English","# Introduction\n## CMAS corrosion impact on turbine TBCs\n## Proposed protection strategies\n### Composition modification\n### Structure modification\n### Surface protective coatings","[{\"question\":\"Why is CMAS attack critical for thermal barrier coatings?\",\"answer\":\"CMAS deposits on blade surfaces, melts at high temperature, penetrates the coating, blocks micropores, and triggers phase transformations and ZrO2 degradation, leading to TBC failure.\"},{\"question\":\"What role do impurity phases in Ti2AlC coatings play?\",\"answer\":\"Ti2AlC coatings contain impurity phases such as TiC and Al2Ti3. With long-term CMAS exposure, these impurities contribute to microstructure degradation and promote the formation of an Al2O3–TiO2 mixed layer rather than a compact Al2O3 layer.\"},{\"question\":\"How does pre-oxidation improve CMAS resistance in Ti2AlC/YSZ TBCs?\",\"answer\":\"Pre-oxidation in air or under controlled oxygen partial pressure increases the formation of a continuous Al2O3 layer on the Ti2AlC surface; an oxygen partial pressure around ~630 Pa is reported to be effective, and a vacuum heat treatment at 867 ℃ for 10 h before pre-oxidation further helps form a compact Al2O3 layer.\"}]","Design of Ti2AlC/YSZ TBCs for more efficient in resisting CMAS attack | PDF",1790964809,48,[147,151,155,159],{"page_no":8,"url":148,"width":149,"height":150},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/59579124881a9e10fda2419bf1068f3c.webp",983,1305,{"page_no":14,"url":152,"width":153,"height":154},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/85db020d6ceca90229726aad4d228bde.webp",982,1304,{"page_no":81,"url":156,"width":157,"height":158},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/7eebda913f94f234c72f92c62da1fafe.webp",981,1303,{"page_no":19,"url":160,"width":161,"height":162},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/a7f123e920ff9c0a7a77b0a52f2e23f2.webp",980,1301]