[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"detail-sidebar-cat-0-en-105":3,"doc-seo-461414-105":59,"doc-detail-461414-en":130},{"code":4,"msg":5,"data":6},0,"success",[7,13,18,23,28,33,38,43,48,51,55],{"id":8,"doc_module":4,"doc_module_name":9,"category_name":10,"show_sort_weight":11,"slug":12},1,"Document","Story & Novel",90,"story-novel",{"id":14,"doc_module":4,"doc_module_name":9,"category_name":15,"show_sort_weight":16,"slug":17},2,"Literature",80,"literature",{"id":19,"doc_module":4,"doc_module_name":9,"category_name":20,"show_sort_weight":21,"slug":22},4,"Exam",70,"exam",{"id":24,"doc_module":4,"doc_module_name":9,"category_name":25,"show_sort_weight":26,"slug":27},5,"Comic",60,"comic",{"id":29,"doc_module":4,"doc_module_name":9,"category_name":30,"show_sort_weight":31,"slug":32},6,"Technology",50,"technology",{"id":34,"doc_module":4,"doc_module_name":9,"category_name":35,"show_sort_weight":36,"slug":37},7,"Healthcare",40,"healthcare",{"id":39,"doc_module":4,"doc_module_name":9,"category_name":40,"show_sort_weight":41,"slug":42},8,"Research & Report",30,"research-report",{"id":44,"doc_module":4,"doc_module_name":9,"category_name":45,"show_sort_weight":46,"slug":47},9,"Religion & Spirituality",20,"religion-spirituality",{"id":46,"doc_module":4,"doc_module_name":9,"category_name":49,"show_sort_weight":46,"slug":50},"World Cup","world-cup",{"id":52,"doc_module":4,"doc_module_name":9,"category_name":53,"show_sort_weight":52,"slug":54},10,"Lifestyle","lifestyle",{"id":56,"doc_module":4,"doc_module_name":9,"category_name":57,"show_sort_weight":24,"slug":58},19,"General","general",{"code":4,"msg":60,"data":61},"ok",{"site_id":62,"language":63,"slug":64,"title":65,"keywords":66,"description":67,"schema_data":68,"social_meta":123,"head_meta":125,"extra_data":127,"updated_unix":129},105,"en","an-in-vitro-analysis-of-surface-treatment-effects-on-the-tensile-bond-strength-between-heat-cured-denture-base-and-heat-polymerized-polymethyl-methacrylate-liner","An In Vitro Analysis of Surface Treatment Effects on the Tensile Bond Strength Between Heat-Cured Denture Base and Heat-Polymerized Polymethyl Methacrylate Liner","","In vitro investigation evaluates how surface conditioning of a heat-cured polymethyl methacrylate (PMMA) denture base affects tensile bond strength with a heat-polymerized PMMA liner. Forty-eight standardized specimens were prepared, sectioned to expose bonding surfaces, and assigned to six conditioning modalities: monomer application, phosphoric acid etching, alumina sandblasting, and combinations including Er,Cr:YSGG laser with either acid or sandblasting, plus an untreated control. Tensile testing after 30 days’ water storage and scanning electron microscopy assessed interface failure modes and microstructural changes.",{"@graph":69,"@context":122},[70,84,105],{"@type":71,"itemListElement":72},"BreadcrumbList",[73,77,79,82],{"item":74,"name":75,"@type":76,"position":8},"https://docshare.wps.com","Home","ListItem",{"item":78,"name":9,"@type":76,"position":14},"https://docshare.wps.com/document/",{"item":80,"name":40,"@type":76,"position":81},"https://docshare.wps.com/document/research-report/",3,{"item":83,"name":65,"@type":76,"position":19},"https://docshare.wps.com/document/an-in-vitro-analysis-of-surface-treatment-effects-on-the-tensile-bond-strength-between-heat-cured-denture-base-and-heat-polymerized-polymethyl-methacrylate-liner/461414/",{"url":83,"name":65,"@type":85,"image":86,"author":91,"headline":65,"publisher":94,"fileFormat":97,"inLanguage":63,"description":67,"dateModified":98,"datePublished":99,"encodingFormat":97,"isAccessibleForFree":100,"interactionStatistic":101},"DigitalDocument",{"url":87,"@type":88,"width":89,"height":90},"https://docshare.wps.com/thumbnails/an-in-vitro-analysis-of-surface-treatment-effects-on-the-tensile-bond-strength-between-heat-cured-denture-base-and-heat-polymerized-polymethyl-methacrylate-liner/461414.png","ImageObject",300,407,{"name":92,"@type":93},"Fans","Person",{"url":74,"name":95,"@type":96},"DocShare","Organization","application/pdf","2026-11-19","2026-09-30",true,{"@type":102,"interactionType":103,"userInteractionCount":39},"InteractionCounter",{"@type":104},"ViewAction",{"@type":106,"mainEntity":107},"FAQPage",[108,114,118],{"name":109,"@type":110,"acceptedAnswer":111},"What was the main goal of this in vitro study?","Question",{"text":112,"@type":113},"To determine how different surface conditioning methods improve interfacial adhesion and tensile bond strength between a heat-cured denture base and a heat-polymerized PMMA liner.","Answer",{"name":115,"@type":110,"acceptedAnswer":116},"How were specimens prepared and grouped?",{"text":117,"@type":113},"Forty-eight heat-cured PMMA specimens were sectioned to expose uniform bonding surfaces and randomly assigned to six groups (n=8), including a no-treatment control and five surface treatment protocols.",{"name":119,"@type":110,"acceptedAnswer":120},"Which surface treatment produced the highest tensile bond strength?",{"text":121,"@type":113},"Methyl methacrylate monomer application showed the highest tensile bond strength, outperforming the other modalities in post-hoc comparisons.","https://schema.org",{"og:url":83,"og:type":124,"og:title":65,"og:site_name":95,"og:description":67},"article",{"robots":126,"canonical":83},"index,follow",{"doc_id":128,"site_id":62},461414,1791165244,{"code":4,"msg":5,"data":131},{"doc_id":128,"user_id":132,"nickname":92,"user_avatar":133,"doc_module":4,"category_id":39,"category_name":40,"doc_title":65,"doc_description":67,"doc_content":134,"file_id":135,"file_url":136,"file_type":137,"file_size":138,"view_count":39,"is_deleted":4,"is_public":8,"is_downloadable":8,"audit_status":8,"page_count":39,"language":139,"language_code":63,"site_id":62,"html_lang":63,"table_of_contents":140,"faqs":141,"seo_title":142,"seo_description":67,"update_tm":143,"read_time":46,"preview_page_count":19,"preview_urls":144},5909892330395,"https://ap-avatar.wpscdn.com/davatar_6f874abed73319feea01a86fa6f0fab8","Review began 11/18/2025  \nReview ended 11/29/2025  \nPublished 12/10/2025  \n© Copyright 2025  \nVerma et al. This is an open access article distributed under the terms of the Creative Commons Attribution License CC-BY 4.0. , which permits unrestricted use , distribution , and reproduction in any medium , provided the original author and source are credited.  \nDOI: 10.7759/cureus.98898  \nOpen Access Original Article  \nAn In Vitro Analysis of Surface Treatment Effects on the Tensile Bond Strength Between HeatCured Denture Base and Heat-Polymerized Polymethyl Methacrylate Liner  \nSumit Verma 1, Manmeet Gulati 1, Manmohit Kumar 1 , Ram R. Goyal 1 , Aalok Mishra 1 , Silky Grover 1, Manish Sharma 2  \n1. Department of Prosthodontics, Desh Bhagat Dental College and Hospital, Mandi Gobindgarh, IND 2. Department of Oral Pathology, Jawahar Medical Foundation 's Annasaheb Chudaman Patil Dental College, Dhule, IND  \nCorresponding author: Sumit Verma, [sumitverma8448@gmail.com](sumitverma8448@gmail.com)  \nAbstract  \nIntroduction: Successful relining of complete dentures requires strong interfacial adhesion between the existing heat-cured polymethyl methacrylate (PMMA) denture base and the newly applied heat-polymerized PMMA liner to prevent delamination under functional stress. This in vitro investigation examined the efficacy of different surface conditioning methods in enhancing bond integrity and microstructural characteristics at the resin-resin interface.  \nMaterials and methods: 48 rectangular specimens were prepared from heat-cured PMMA resin and subjected to standardized long-cycle polymerization. Each specimen was sectioned at the midline to expose a uniform bonding surface and randomly allocated to six experimental groups (n = 8): no treatment (control), methyl methacrylate monomer application, 36% phosphoric acid etching, 50 µm alumina particle sandblasting, erbium, chromium, yttrium-scandium-gallium-garnet (Er,Cr:YSGG) laser irradiation followed by phosphoric acid etching, and laser irradiation followed by alumina sandblasting. All procedures used calibrated equipment, digital timing, and custom positioning jigs to ensure reproducibility. The liner was applied using an identical resin from the same batch, trial-packed under controlled pressure, and polymerized using the same technique. The specimens were stored in distilled water for 30 days before testing. The tensile bond strength was determined by three-point bending using a universal testing machine. The selected samples underwent gold sputter coating and examination using field-emission scanning electron microscopy.  \nResults: The tensile bond strength varied significantly across groups (p \u003C 0 .001) . The untreated control recorded the lowest mean tensile strength at 0.92 ± 0.06 megapascals (MPa) . Monomer application achieved the highest value of 1 .89 ± 0.04 MPa, followed by laser plus phosphoric acid at 1.74 ± 0.03 MPa, laser plus sandblasting at 1.41 ± 0.04 MPa, sandblasting alone at 1.24 ± 0.03 MPa, and phosphoric acid alone at 1.15 ± 0.02 MPa. Post-hoc comparisons confirmed the statistical superiority of the monomer group over all other modalities, and positioned the laser-phosphoric acid combination as the next most effective approach. Scanning electron microscopy revealed smooth, non-retentive control surfaces with adhesive failure, whereas monomer-treated interfaces displayed polymer interdiffusion and cohesive failure. Laserphosphoric acid samples exhibited deep micro-undercuts with extensive resin penetration, whereas sandblasting produced superficial grooves with incomplete infiltration.  \nConclusion: Monomer application was found to be the most reliable and clinically practical method for maximizing liner adhesion through chemical interpenetration. The laser phosphoric acid protocol provides a viable alternative when advanced equipment is available, combining precise ablation with enhanced wettability.  \nCategories: Dentistry  \nKeywords: liner, polymethyl methacr","cbCaicZc2ft2lL7S","https://ap.wps.com/l/cbCaicZc2ft2lL7S","pdf",2127622,"English","# Abstract\n# Introduction\n# Materials and methods\n# Results\n# Conclusion\n# How to cite this article\n# Surface treatments","[{\"question\":\"What was the main goal of this in vitro study?\",\"answer\":\"To determine how different surface conditioning methods improve interfacial adhesion and tensile bond strength between a heat-cured denture base and a heat-polymerized PMMA liner.\"},{\"question\":\"How were specimens prepared and grouped?\",\"answer\":\"Forty-eight heat-cured PMMA specimens were sectioned to expose uniform bonding surfaces and randomly assigned to six groups (n=8), including a no-treatment control and five surface treatment protocols.\"},{\"question\":\"Which surface treatment produced the highest tensile bond strength?\",\"answer\":\"Methyl methacrylate monomer application showed the highest tensile bond strength, outperforming the other modalities in post-hoc comparisons.\"}]","An In Vitro Analysis of Surface Treatment Effects on the Tensile Bond Strength Between Heat-Cured Denture Base and Heat-Polymerized Polymethyl Methacrylate Liner | PDF",1790761551,[145,149,153,157],{"page_no":8,"url":146,"width":147,"height":148},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/665bff679716dd23e9bf539ae731fc14.webp",983,1390,{"page_no":14,"url":150,"width":151,"height":152},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/24cd7175b7e35aadb427d7904490d805.webp",982,1389,{"page_no":81,"url":154,"width":155,"height":156},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/1ec0800f5edfe4fe1dd87a4b7bc2c65f.webp",981,1387,{"page_no":19,"url":158,"width":159,"height":160},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-17/453dcc36c2a73ac1334a93fc397cd156.webp",980,1386]