[{"data":1,"prerenderedAt":-1},["ShallowReactive",2],{"doc-seo-760935-105":3,"detail-sidebar-cat-0-en-105":79,"doc-detail-760935-en":129},{"code":4,"msg":5,"data":6},0,"ok",{"site_id":7,"language":8,"slug":9,"title":10,"keywords":11,"description":12,"schema_data":13,"social_meta":72,"head_meta":74,"extra_data":76,"updated_unix":78},105,"en","alfaterxl-injection-molding-processing-guide","ALFATERXL - Injection Molding Processing Guide","","ALFATERXL® is a PP-based thermoplastic vulcanizate (TPV) with cross-linked EPDM, supplied in multiple injection molding series tailored to different applications. The guide explains why TPV processing differs from conventional thermoplastics and provides practical first-step recommendations for customers with limited TPV experience. It covers drying requirements, the impact of shear rate and temperature on flow and viscosity, flowability differences across series, spiral flow guidance, anisotropic shrinkage behavior with ISO references, and key processing parameters affecting shrinkage, plus recommended machinery and temperature profiles.",{"@graph":14,"@context":71},[15,34,54],{"@type":16,"itemListElement":17},"BreadcrumbList",[18,23,27,31],{"item":19,"name":20,"@type":21,"position":22},"https://docshare.wps.com","Home","ListItem",1,{"item":24,"name":25,"@type":21,"position":26},"https://docshare.wps.com/document/","Document",2,{"item":28,"name":29,"@type":21,"position":30},"https://docshare.wps.com/document/technology/","Technology",3,{"item":32,"name":10,"@type":21,"position":33},"https://docshare.wps.com/document/alfaterxl-injection-molding-processing-guide/760935/",4,{"url":32,"name":10,"@type":35,"image":36,"author":41,"headline":10,"publisher":44,"fileFormat":47,"inLanguage":8,"description":12,"dateModified":48,"datePublished":48,"encodingFormat":47,"isAccessibleForFree":49,"interactionStatistic":50},"DigitalDocument",{"url":37,"@type":38,"width":39,"height":40},"https://docshare.wps.com/thumbnails/alfaterxl-injection-molding-processing-guide/760935.png","ImageObject",300,407,{"name":42,"@type":43},"River Wang","Person",{"url":19,"name":45,"@type":46},"DocShare","Organization","application/pdf","2026-11-29",true,{"@type":51,"interactionType":52,"userInteractionCount":22},"InteractionCounter",{"@type":53},"ViewAction",{"@type":55,"mainEntity":56},"FAQPage",[57,63,67],{"name":58,"@type":59,"acceptedAnswer":60},"Is ALFATERXL® hygroscopic, and how should it be dried before molding?","Question",{"text":61,"@type":62},"ALFATERXL® injection molding series are basically non-hygroscopic. Drying for 2–4 hours at 70–80 °C in a dry-air dryer is recommended to remove surface moisture, and open bags should not be stored long-term.","Answer",{"name":64,"@type":59,"acceptedAnswer":65},"How do shear rate and temperature affect the flow behavior of ALFATERXL®?",{"text":66,"@type":62},"ALFATERXL® viscosity is more sensitive to shear than to heat. Higher injection speed increases shear rate, which lowers viscosity and supports easier flowing, while temperature increases have only a moderate effect on flowability.",{"name":68,"@type":59,"acceptedAnswer":69},"What is shrinkage behavior and what factors influence it?",{"text":70,"@type":62},"ALFATERXL® shrinkage is anisotropic, shrinking differently along flow direction versus transverse to flow direction, and softer grades tend to shrink more. Shrinkage values depend strongly on injection molding conditions and part design, and can be optimized by adjusting parameters such as injection speed, holding pressure/time, mold temperature, and cooling time.","https://schema.org",{"og:url":32,"og:type":73,"og:title":10,"og:site_name":45,"og:description":12},"article",{"robots":75,"canonical":32},"index,follow",{"doc_id":77,"site_id":7},760935,1795949918,{"code":4,"msg":80,"data":81},"success",[82,86,90,94,99,103,108,113,118,121,125],{"id":22,"doc_module":4,"doc_module_name":25,"category_name":83,"show_sort_weight":84,"slug":85},"Story & Novel",90,"story-novel",{"id":26,"doc_module":4,"doc_module_name":25,"category_name":87,"show_sort_weight":88,"slug":89},"Literature",80,"literature",{"id":33,"doc_module":4,"doc_module_name":25,"category_name":91,"show_sort_weight":92,"slug":93},"Exam",70,"exam",{"id":95,"doc_module":4,"doc_module_name":25,"category_name":96,"show_sort_weight":97,"slug":98},5,"Comic",60,"comic",{"id":100,"doc_module":4,"doc_module_name":25,"category_name":29,"show_sort_weight":101,"slug":102},6,50,"technology",{"id":104,"doc_module":4,"doc_module_name":25,"category_name":105,"show_sort_weight":106,"slug":107},7,"Healthcare",40,"healthcare",{"id":109,"doc_module":4,"doc_module_name":25,"category_name":110,"show_sort_weight":111,"slug":112},8,"Research & Report",30,"research-report",{"id":114,"doc_module":4,"doc_module_name":25,"category_name":115,"show_sort_weight":116,"slug":117},9,"Religion & Spirituality",20,"religion-spirituality",{"id":116,"doc_module":4,"doc_module_name":25,"category_name":119,"show_sort_weight":116,"slug":120},"World Cup","world-cup",{"id":122,"doc_module":4,"doc_module_name":25,"category_name":123,"show_sort_weight":122,"slug":124},10,"Lifestyle","lifestyle",{"id":126,"doc_module":4,"doc_module_name":25,"category_name":127,"show_sort_weight":95,"slug":128},19,"General","general",{"code":4,"msg":80,"data":130},{"doc_id":77,"user_id":131,"nickname":42,"user_avatar":132,"doc_module":4,"category_id":100,"category_name":29,"doc_title":10,"doc_description":12,"doc_content":133,"file_id":134,"file_url":135,"file_type":136,"file_size":137,"view_count":22,"is_deleted":4,"is_public":22,"is_downloadable":22,"audit_status":22,"page_count":122,"language":138,"language_code":8,"site_id":7,"html_lang":8,"table_of_contents":139,"faqs":140,"seo_title":141,"seo_description":12,"update_tm":78,"read_time":142,"preview_page_count":33,"preview_urls":143},1099514067438,"https://ap-avatar.wpscdn.com/avatar/100002539ee87300030?x-image-process=image/resize,m_fixed,w_180,h_180&k=1780474512215547542","Injection Molding Grades  \nPROCESSING GUIDE  \nALFATERXL® is a thermoplastic vulcanizate (TPV) based on PP and cross-linked EPDM. Different ALFATERXL® series are available and optimized for various injection molding applications:  \n• ALFATERXL® I 2GP series  \n• ALFATERXL® I 3EF series  \n• ALFATERXL® I 4GP series  \n• ALFATERXL® I 4FC series  \n• ALFATERXL® I 4PA series  \nTypical injection molding applications are shown in Figure 1. Processing of TPV is generally different from conventional thermoplastics. The following injection molding guidelines aim to provide a first support, especially for customers with less experience in TPV processing.  \nFigure 1: Gaskets produced by injection molding.  \nFigure 1: Mud flaps produced by injection molding.  \nDRYING  \nThe ALFATERXL® injection molding series are basically non-hygroscopic . However, drying for 2 – 4 hours at  \n70 – 80 °C in a dry-air dryer is recommended to remove any surface moisture. Open bags should not be stored over a long period of time.  \nFLOWABILITY AND SHRINKAGE  \nHarder ALFATERXL® grades have basically higher viscosity than softer grades. The viscosity of ALFATERXL® is more sensitive to shear than to heat (Figure 2) . Appropriate flow, homogeneity, and molding behavior of the ALFATERXL® melt is achieved by applying sufficiently high shear.  \nPage 1 of 10  \nTherefore, appropriate injection molding parameters and gate design are required. In general, the faster the injection speed, the higher the shear rate and the lower the viscosity (= easier flowing) . In contrast, temperature increases have only a moderate effect on the flowability and molding behavior of the ALFATERXL® melt.  \nInfluence of shear rate on viscosity  \nV iscos ity ( Pa ·s)  \n10.000  \n1.000  \n100  \n10  \n1  \n\n| ~~  ~~  ALFATER XL® (low hardness)\u003Cbr>  ALFATER XL® (high hardness) |  |\n| --- | --- |\n| \u003Cbr>\u003Cbr>\u003Cbr>\u003Cbr>\u003Cbr>Typical shear rate range for injection molding |  |\n|  |  |\n|  |  |\n\n10 100 1.000 10.000 100.000  \nShear rate (1/s)  \nFigure 2: Influence of shearing and temperature on the flow behavior (viscosity) of ALFATERXL® melt.  \nInfluence of temperature on viscosity  \nV iscos ity ( Pa ·s)  \n50  \n40  \n30  \n20  \n10  \n0  \nALFATERXL® A70I 2GP0050 BK0002-00 Viscosity at shear rate: 5000 1/s  \n185 190 195 200 205 210 215  \nTemperature (°C)  \nPage 2 of 10  \nThe ALFATERXL® injection molding series provide different flowability. Therefore not all series are suitable for the same molding part or application . The following table provides a short overview about the general flow behavior and potential use of the ALFATERXL® injection molding series .  \n\n| Material | Flowability | Spiral flow*(2 mm thickness) | Characteristics |\n| --- | --- | --- | --- |\n| ALFATERXL® I 2GP series | normal flow | \u003C 50 cm | Standard injection molding series, standard molding parts, flow length ≤ 150 mm, best tensile properties and compression set |\n| ALFATERXL® I 3EF series | easy flow | > 50 cm | Thin-walled parts, complex part designs, flow length > 150 mm, excellent weathering resistance |\n| ALFATERXL® I 4GP series | easy flow | > 50 cm | Thin-walled parts, complex part designs, flow length > 150 mm, natural and bright colored parts, low emission parts |\n| ALFATERXL® I 4FC series | easy flow | > 50 cm | Thin-walled parts, complex part designs, flow length > 150 mm, parts for food contact |\n\n* Spiral flow: thickness 2 mm, melt temperature 220 °C, mold temperature 70 °C, injection pressure 500 bar  \nShrinkage of ALFATERXL® is anisotropic (shrinks differently in flow direction and transverse to flow direction) . Softer ALFATERXL® grades tend to shrink more than harder grades . Shrinkage depends strongly on the injection molding conditions and part design . The shrinkage values for the ALFATERXL® injection molding series given below have been measured on standard sample plaques and are therefore only a guideline. Depending on the injection molding process, the processing conditions and the part design, these values can vary.  \n\n| H","cbCaiaWRQn24TojI","https://ap.wps.com/l/cbCaiaWRQn24TojI","pdf",151683,"English","# Drying\n# Flowability and Shrinkage\n## Influence of Shear Rate on Viscosity\n## Influence of Temperature on Viscosity\n# Material Series Overview\n# Machinery and Equipment\n# Temperature Profile","[{\"question\":\"Is ALFATERXL® hygroscopic, and how should it be dried before molding?\",\"answer\":\"ALFATERXL® injection molding series are basically non-hygroscopic. Drying for 2–4 hours at 70–80 °C in a dry-air dryer is recommended to remove surface moisture, and open bags should not be stored long-term.\"},{\"question\":\"How do shear rate and temperature affect the flow behavior of ALFATERXL®?\",\"answer\":\"ALFATERXL® viscosity is more sensitive to shear than to heat. Higher injection speed increases shear rate, which lowers viscosity and supports easier flowing, while temperature increases have only a moderate effect on flowability.\"},{\"question\":\"What is shrinkage behavior and what factors influence it?\",\"answer\":\"ALFATERXL® shrinkage is anisotropic, shrinking differently along flow direction versus transverse to flow direction, and softer grades tend to shrink more. Shrinkage values depend strongly on injection molding conditions and part design, and can be optimized by adjusting parameters such as injection speed, holding pressure/time, mold temperature, and cooling time.\"}]","ALFATERXL - Injection Molding Processing Guide | PDF",25,[144,148,152,156],{"page_no":22,"url":145,"width":146,"height":147},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-29/36901916fcc69a6d918cb833be895d31.webp",983,1390,{"page_no":26,"url":149,"width":150,"height":151},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-29/49414876a06a08420ad825dae19bb0c7.webp",982,1388,{"page_no":30,"url":153,"width":154,"height":155},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-29/cef7823f287d106019d6298d3995765f.webp",981,1387,{"page_no":33,"url":157,"width":158,"height":159},"https://res-academy.cache.wpscdn.com/upload/kdocshare/2026-11-29/12ec8acd4e08c0e9a778e3dd196c4162.webp",980,1385]